Open-die forging works, Jiangyin, Jiangsu, China. Rings, flanges, shafts, discs, sleeves. Tel +86-189-2135-9659 | sales@steelforgepieces.com
JJM Jiangyin Jiangnan Metal Co., Ltd. Melting works, open-die forge and ring mill since 1997

Z15CNS25-20 Forgings (X15CrNiSi25-21 / 1.4841 / AISI 314 / UNS S31400)

Open-die forged rings, seamless rolled rings, flanges, shafts, discs, sleeves, bushings, tube sheets and bars, made to drawing by Jiangyin Jiangnan Metal Co., Ltd.

Jiangyin Jiangnan Metal Co., Ltd., melting works and open-die forge, Jiangyin, Jiangsu, China. Updated . Reference standards: EN 10095, EN 10088-3, SEW 470, EN 10204, EN 10228-3, ASTM A388, SEP 1921.

Z15CNS25-20, also written Z15CNS25.20, is the French AFNOR designation for an austenitic chromium-nickel-silicon heat-resisting steel of roughly 24-26 % Cr, 19-21 % Ni and 1.5-2.5 % Si. The European equivalent is X15CrNiSi25-21, material number 1.4841, and the American equivalent is AISI 314 / UNS S31400. The high silicon level lifts scaling resistance in air to about 1150 °C, which is why the grade turns up in furnace internals, refinery hardware and thermal processing equipment. We melt the steel on site, forge it to drawing and supply it solution annealed with EN 10204 3.1 or 3.2 certification.

AFNORZ15CNS25-20
EN / WerkstoffX15CrNiSi25-21 / 1.4841
AISI / UNS314 / S31400
StructureAustenitic
Scaling resistanceapprox. 1150 °C in air
Forging range1175-1000 °C

1. The grade

Z15CNS25-20 belongs to the family of high-alloy chromium-nickel-silicon steels used where parts have to hold shape in hot oxidising gas. The AFNOR code reads directly: Z for high-alloy steel, 15 for a nominal 0.15 % carbon, C-N-S for chromium, nickel and silicon, and 25-20 for the nominal chromium and nickel levels.

Silicon is what separates this grade from plain 25Cr-20Ni material such as 310S. It builds a tighter oxide film, so the useful limit in air rises to roughly 1150 °C, with continuous service usually planned at about 1100 °C to leave margin. Creep resistance is useful to around 690 °C. The picture changes in sulphur-bearing atmospheres, where published data for 1.4841 puts the ceiling near 650 °C in oxidising and reducing sulphurous gases.

The structure is fully austenitic, so the steel cannot be hardened by quenching or by ageing. Strength comes from the alloy content and from grain size set during forging and annealing.

2. Equivalent designations

Z15CNS25-20 cross reference
Standard / countryDesignation
AFNOR, FranceZ15CNS25-20, also written Z15CNS25.20. Related: Z10CNS25-20
EN, EuropeX15CrNiSi25-21, material number 1.4841
SEW 470, GermanyX15CrNiSi25-20 (1.4841)
AISI / SAE / UNS, USA314, SAE 314, S31400
BS, United Kingdom314S25
JIS, JapanSUH 310
PN, PolandH25N20S2
GOST, Russia20Kh25N20S2
UNE, SpainF-3310
CSN, Czech Republic17255

Cross references show the closest known equivalents. Chemistry limits differ slightly between standards, so check the governing specification before substituting one for another.

Watch the near grades. Z15CNS25-20 / 1.4841 is often mixed up with 310 and 310S (1.4845, X8CrNi25-21), which share the Cr-Ni base but carry far less silicon and therefore less scaling resistance. One step down is 1.4828 / AISI 309 (X15CrNiSi20-12), good to roughly 950-1000 °C. If your drawing allows an alternative, tell us the working temperature and the atmosphere and we will say which grade makes sense for the money.

3. Chemical composition

Composition, mass fraction in %
ElementZ15CNS25-20 (AFNOR)X15CrNiSi25-21 / 1.4841 (EN)
Carbon, Cmax 0.15max 0.20
Silicon, Si1.50 to 2.501.50 to 2.50
Manganese, Mnmax 2.00max 2.00
Phosphorus, Pmax 0.040max 0.045
Sulphur, Smax 0.015max 0.015
Chromium, Cr24.0 to 26.024.0 to 26.0
Nickel, Ni19.0 to 21.019.0 to 22.0
Nitrogen, Nnot specifiedmax 0.11
Iron, Febalancebalance

Some mill data sheets for 1.4841 quote a narrower silicon band of 1.50 to 2.00 %. Ladle analysis of the actual heat is issued with every certificate.

4. Mechanical properties

Room temperature values, solution annealed, bar up to 160 mm diameter
PropertyMetricImperial
Tensile strength Rm550 to 750 MPa80 to 109 ksi
Proof strength Rp0.2min 230 MPamin 33 ksi
Proof strength Rp1.0min 270 MPamin 39 ksi
Elongation A5, longitudinalmin 30 %min 30 %
Hardnessmax 223 HBabout max 20 HRC
Modulus of elasticity196 GPa28.4 x 106 psi

Figures apply to the equivalent grade 1.4841 in the solution annealed condition. Acceptance values for a given forging depend on section size, test location and the purchase specification, and are agreed before production starts.

5. Physical and creep data

Physical properties at 20 °C
PropertyValue
Density7.9 g/cm³
Thermal conductivity15 W/m·K
Specific heat capacity500 J/kg·K
Electrical resistivity0.90 Ω·mm²/m at 20 °C, 1.25 Ω·mm²/m at 1000 °C
Linear expansion15.2 x 10-6 K-1 for 20-100 °C, rising to 19.5 x 10-6 K-1 for 20-1200 °C
Magnetic behaviourpractically non-magnetic when annealed, slightly magnetic after cold work
Creep rupture strength, MPa, for guidance only
Temperature1 000 h10 000 h100 000 h
600 °C17013080
700 °C904018
800 °C40207
900 °C20103
1000 °C5--

Creep values are design guidance for the equivalent grade 1.4841 and are not guaranteed properties of a delivered forging.

6. Forging, annealing, welding, machining

Forging

The grade forges well. Published practice for 1.4841 gives a range of 1175 °C down to 1000 °C with rapid cooling in air or water afterwards, and some mill data allows hot work down to 800 °C with air cooling. Open-die and closed-die work are both possible. On our presses and hammers we keep the finishing temperature above the recrystallisation range so the structure stays even, and we set reduction ratios so the centre of a heavy section is genuinely worked rather than only upset.

Heat treatment

Solution annealing runs at roughly 1050 to 1150 °C with fast cooling in water, or in air for thin sections. There is no hardening or ageing step, because the grade is austenitic. If a specification calls for solution plus ageing on this material, it needs reviewing before we cut steel. Keep parts out of the 600 to 900 °C band for long periods, since sigma phase forms there and takes ductility with it.

Welding

TIG, MAG, submerged arc, laser and manual arc all work. Preheating is not normally needed and no post-weld heat treatment is required, but heat input should be held down because hot cracking is a risk. The usual filler is 1.4842 (X12CrNi25-20). Corrosion resistance drops after welding and the as-welded material is open to intergranular attack.

Machining

Machinability is medium. Carbides wear tools, thermal conductivity is low and the surface work-hardens, so moderate speeds, a positive depth of cut and plenty of coolant pay off.

7. Forged products in Z15CNS25-20

Everything below is produced to the customer's drawing or specification. We do not hold a fixed catalogue of finished items in this grade.

Product forms
FormScope
Seamless rolled rings and forged ringsRing rolling and mandrel forging, plain, stepped or contoured sections
Forged flangesWeld neck, blind, slip-on, long weld neck and special profiles
Shafts, spindles, eccentric shafts, crankshaftsSolid and stepped shafts, upset ends
Discs, disks, blanksFlat and profiled discs, gear blanks, hubs
Sleeves, bushings, hollow barsTrepanned or bored hollows, see our forged sleeves
Tubes, pipes, tube sheetsHeavy wall hollow forgings, tube sheets drilled or undrilled
Round bars, square bars, blocksHot forged, peeled, turned or ground
Valve componentsBodies, bonnets, stems, seat rings, blocks, nozzles

Delivery conditions include as forged, rough machined with allowance, finish machined to drawing, solution annealed, pickled or shot blasted. Melting routes available for this grade are EF with LF and VOD refining, and ESR where the specification asks for lower inclusion content.

8. Applications

Furnace construction, apparatus engineering and petrochemical plant are the main fields for 1.4841 and its equivalents, along with pyrolysis and methane conversion equipment, furnace conveyors and hooks, and glass industry tooling.

Orders we see most often for this grade cover fluidised bed furnace internals, grids, wind boxes and coal combustor parts; smelter and continuous casting equipment in ore processing and steel plants; recuperators, tube hangers, flares and catalytic recovery components in refineries, including fluid catalytic cracking units and polythionic acid service; burners, burner shields and feed or discharge systems in sintering and cement plants; annealing boxes and covers, muffles, retorts, fans, doors and walking beams in thermal processing; and shell and tube heat exchangers, columns, towers, silos and preheaters in process plant.

9. Testing and certification

Ultrasonic testing is carried out to EN 10228-3, SEP 1921 or ASTM A388, with the acceptance class fixed on the order. We also provide ladle and product analysis, tensile, impact and hardness testing, intergranular corrosion testing, PMI, liquid penetrant examination, grain size determination and dimensional reports. Certificates are issued to EN 10204 3.1, or to EN 10204 3.2 countersigned by a third party such as TUV, SGS, BV or Lloyd's when the contract calls for it. The works holds CCS, BV, DNV, LR and NK approvals.

10. Questions we get asked

What is Z15CNS25-20 steel?
An austenitic chromium-nickel-silicon heat-resisting steel under the French AFNOR system, roughly 24-26 % Cr, 19-21 % Ni and 1.5-2.5 % Si. European equivalent X15CrNiSi25-21 / 1.4841, American equivalent AISI 314 / UNS S31400.
What is the equivalent of Z15CNS25-20?
X15CrNiSi25-21 (1.4841), SEW 470 X15CrNiSi25-20, AISI and SAE 314, UNS S31400, BS 314S25, JIS SUH310, PN H25N20S2, GOST 20Kh25N20S2, UNE F-3310, CSN 17255.
How hot can it run?
About 1150 °C for scaling resistance in air, with continuous duty normally planned near 1100 °C. Sulphur-bearing gas pulls the limit back to roughly 650 °C. Avoid long exposure between 600 and 900 °C because of sigma phase.
Can it be hardened?
No. It is fully austenitic, so neither quenching nor ageing raises hardness. Standard delivery condition is solution annealed at 1050 to 1150 °C with fast cooling.
Is it the same as 310S?
No. Both are 25Cr-20Ni austenitics, but this grade carries 1.5 to 2.5 % silicon for better oxidation resistance, while 310S (1.4845) has much less silicon and lower carbon. Pick on service temperature, atmosphere and whether intergranular corrosion matters.
Minimum quantity and lead time?
Single prototype pieces and series orders are both fine, from 10 kg upwards with no minimum piece count. Lead time normally runs 20 to 60 days depending on material availability, forging weight and machining content, and is confirmed with each quotation. Send dimensions or a drawing to sales@steelforgepieces.com for a firm answer.
Who makes these forgings?
Jiangyin Jiangnan Metal Co., Ltd., a melting works and open-die forge at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Telephone +86-189-2135-9659, email sales@steelforgepieces.com.

11. Enquiry

Send a drawing, a sketch with dimensions, or just outside diameter, inside diameter, height and quantity. If the grade is still open, add the service temperature and the medium and we will tell you whether Z15CNS25-20 is the right call or whether another heat-resisting grade does the job for less.

sales@steelforgepieces.com   +86-189-2135-9659

Jiangyin Jiangnan Metal Co., Ltd., melting works and open-die forge
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel +86-189-2135-9659, email sales@steelforgepieces.com