XM-29 Forgings, UNS S24000 / Nitronic 33
Open die forged rings, seamless rolled rings, flanges, round bars, shafts, discs, sleeves, bushings and tube sheets in nitrogen strengthened austenitic stainless steel.
XM-29 at a glance
XM-29 is the ASTM designation for UNS S24000, a nitrogen strengthened austenitic stainless steel with 17.00 to 19.00 % Cr, 11.50 to 14.50 % Mn, 2.25 to 3.75 % Ni and 0.20 to 0.40 % N. The same grade is sold under the trade name Nitronic 33 and by Carpenter Technology as 18Cr-3Ni-12Mn. Manganese and nitrogen take the place of most of the nickel used in Type 304, which gives an annealed yield strength about twice that of 304 together with good toughness, good ductility and very low magnetic permeability that is held after severe cold work and at cryogenic temperature.
Bar to ASTM A276 Type XM-29 must meet 100 ksi (690 MPa) tensile, 55 ksi (380 MPa) yield, 30 % elongation and 50 % reduction of area as minimum values. The grade hardens by cold work only and does not respond to thermal hardening.
Jiangyin Jiangnan Metal Co., Ltd. is an open die forging factory in Jiangyin, Jiangsu, China that makes XM-29 forgings to customer drawings, with forging stock ordered to ASTM A314. Enquiries go to sales@steelforgepieces.com or +86-189-2135-9659.
Datasheet reviewed 11 October 2026 by the metallurgical department of Jiangyin Jiangnan Metal Co., Ltd.
1. What XM-29 is
XM-29 belongs to the Cr-Mn-N austenitic family. Instead of 8 to 10 % nickel, austenite is held stable by roughly 12 % manganese together with 0.20 to 0.40 % nitrogen in solid solution. Nitrogen is an effective strengthener, so the grade reaches its high yield strength in the annealed condition rather than through cold work or precipitation hardening. The manganese level raises hot ductility and allows the steel to dissolve more nitrogen than a conventional 18-8 composition can hold.
Because the austenite is stable, the structure does not transform to martensite under heavy deformation or at low temperature. That is the reason the grade keeps very low magnetic permeability after severe cold working and down to cryogenic temperature, and it is the property behind most non-magnetic applications.
Designation cross reference
| Designation type | Value |
|---|---|
| UNS | S24000 |
| ASTM type symbol | XM-29, tubular products TP XM-29 |
| Trade name | Nitronic 33 |
| Producer designation | Carpenter 18Cr-3Ni-12Mn |
| SAE | XM-290 |
| ASTM product specifications | A240 plate, sheet and strip; A276 bars and shapes; A249; A269; A312; A358; A412; A479; A580; A688; A813; A814 |
| Forging stock | ASTM A314, stainless steel billets and bars for forging |
2. Chemical composition of XM-29 (UNS S24000)
| Element | Content (%) | Function |
|---|---|---|
| Carbon, C | 0.08 max | Held low to limit carbide precipitation |
| Silicon, Si | 0.75 max, 1.00 max in ASTM A276 | Deoxidiser |
| Manganese, Mn | 11.50 to 14.50 | Austenite stabiliser, raises nitrogen solubility and hot ductility |
| Phosphorus, P | 0.060 max | Residual |
| Sulfur, S | 0.030 max | Residual |
| Chromium, Cr | 17.00 to 19.00 | Passive film, corrosion resistance |
| Nickel, Ni | 2.25 to 3.75, listed as 2.3 to 3.7 in ASTM A276 and A240 | Austenite stability, toughness |
| Nitrogen, N | 0.20 to 0.40 | Main solid solution strengthener |
| Iron, Fe | Balance | Base |
Forging stock is procured from EAF plus VOD or ESR melted heats. The melting route is stated on the mill certificate issued with every order.
3. Mechanical properties
3.1 Specified minimum values
| Property | ASTM A276 Type XM-29 bar, hot and cold finished | ASTM A240 UNS S24000 plate |
|---|---|---|
| Tensile strength, min | 100 ksi (690 MPa) | 690 MPa |
| Yield strength, min | 55 ksi (380 MPa) | 415 MPa |
| Elongation in 2 in. or 4D, min | 30 % | 40 % |
| Reduction of area, min | 50 % | not specified |
3.2 Typical annealed values
| Property | Metric | Imperial |
|---|---|---|
| Tensile strength | 689 MPa typical, up to about 770 MPa reported | 100 ksi, up to about 110 ksi |
| Yield strength, 0.2 % proof | 379 MPa typical, up to about 430 MPa reported | 55 ksi, up to about 63 ksi |
| Elongation at break in 2 in. | 39 to 40 % | 39 to 40 % |
| Reduction of area | about 57 % | about 57 % |
| Hardness, Brinell | 210 to 241 HB | 210 to 241 HB |
| Hardness, Rockwell B | 88 to 100 HRB | 88 to 100 HRB |
| Modulus of elasticity | 200 GPa | 29 x 106 psi |
| Shear modulus | 77 GPa | 11 x 106 psi |
| Shear strength | 530 MPa | 77 ksi |
| Fatigue strength | 370 MPa | 54 ksi |
| Poisson ratio | 0.28 | 0.28 |
4. Physical and thermal properties
| Property | Metric | Imperial |
|---|---|---|
| Density | 7.775 g/cm³ | 0.2808 lb/in³ |
| Thermal expansion coefficient, 26 to 93 C (78 to 200 F) | 16.074 µm/m·C | 8.93 µin/in·F |
| Specific heat capacity | 480 J/kg·K | 0.12 BTU/lb·F |
| Melting onset, solidus | 1350 C | 2460 F |
| Melting completion, liquidus | 1390 C | 2540 F |
| Latent heat of fusion | 280 J/g | not applicable |
| Magnetic permeability | Very low, held after severe cold work and at cryogenic temperature | |
5. XM-29 compared with Type 304
XM-29 is superior to Type 304 in five specific points.
- Yield strength in the annealed condition is about twice that of 304, which allows thinner and lighter sections for the same design load.
- Strength and ductility at cryogenic temperature are excellent, with no deformation induced martensite to embrittle the structure.
- Resistance to stress corrosion cracking is better than 304. The margin over 304 and 304L in hot chloride solutions is clear at lower stress levels; at about 50 ksi and above the two grades are equal.
- Low magnetic permeability is held at cryogenic temperature and after severe cold working.
- Resistance to wear and galling is better than the standard austenitic stainless steels.
Nickel content of about 3 % instead of 8 to 10 % also keeps the grade less exposed to nickel price movement, and base metal cost is moderately low among wrought austenitic stainless steels.
6. Corrosion resistance and service limits
General corrosion resistance of XM-29 is superior to Type 409 and close to Type 304. In weak acid solutions it approaches 304. In more aggressive media it is somewhat less resistant than 304.
7. Forging, heat treatment and fabrication
7.1 Forging practice
The stock is heated to 1093 C (2000 F) and soaked until the section has equalized, then heated again to 1177 C (2150 F) and equalized before forging. The two stage heat avoids thermal gradients in heavy sections, and the high finishing temperature is needed because nitrogen strengthened austenite is considerably stiffer at temperature than 18-8 grades.
7.2 Solution annealing
After forging the parts are soaked at 1038 to 1121 C (1900 to 2050 F) and then rapidly quenched in water or air.
7.3 Forming, machining, welding and hardening
| Operation | Practice |
|---|---|
| Forming | Commonly used forming methods apply. Process annealing at about 1065 C (1950 F) removes the stress that builds up because of the high work hardening rate. |
| Machining | Slow speeds, positive feeds and a resulphurised lubricant are recommended. Chips can be stringy and tough, so chip breakers or curlers are useful. |
| Welding | Submerged arc welding, gas metal arc welding and gas tungsten arc welding are all used. The same equipment and techniques as conventional austenitic grades generally apply. |
| Hardening | By cold work only. The grade cannot be hardened by thermal treatment. |
8. XM-29 forged product forms
All items below are produced by open die forging or ring rolling to the customer drawing, supplied solution annealed unless another condition is agreed.
| Product form | Typical use |
|---|---|
| Forged rings and seamless rolled rings | Containment rings, retaining rings, non-magnetic structural rings |
| Forged flanges and flange blanks | Piping and pressure containing connections |
| Forged round bars, square bars and billets | Machining stock, fasteners, pins, valve stems |
| Forged shafts, spindles and eccentric shafts | Rotating equipment that requires low magnetic permeability |
| Forged discs, disks and tube sheets | Heat exchanger and vessel internals |
| Forged sleeves, bushings and hollow bars | Wear and galling resistant bushings |
| Forged tubes, pipes and nozzles | Tube assemblies and pipework components |
| Forged valve bodies, seat rings, blocks and valve parts | Ball, gate, globe, check and plug valves, strainers |
| Forged gears, rolls, wheels and manifolds | Mechanical and structural components |
9. Typical applications
Published applications for this grade include tube assemblies, pipes, cable, valves, tanks, containment rings and fans. In practice the grade is specified when a project needs a non-magnetic austenitic structure that survives heavy cold work, about double the annealed yield strength of 304 at a lower nickel content, dependable toughness at cryogenic temperature, or better galling and wear behaviour than standard austenitic grades.
Those requirements lead to forged XM-29 parts in cryogenic and liquefied gas equipment, generator and electrical hardware where magnetic permeability must stay low, bulk solid handling and screening equipment, hoppers, chutes and trailer bed liners where wear matters, wastewater and sewage treatment structures, and general mechanical and structural parts that need more strength than 304 can give. For chloride rich or seawater duty see the service limit in section 6.
10. Testing, inspection and certification
- Chemical analysis and room temperature tensile test on every heat, with hardness and, on request, Charpy impact and cryogenic testing.
- Ultrasonic examination to EN 10228-3, SEP 1921 or ASTM A388 as nominated on the purchase order.
- Dimensional inspection against the customer drawing, with PMI and liquid penetrant testing on request.
- Material certification to EN 10204 3.1, or EN 10204 3.2 endorsed by a third party such as TUV, BV, DNV or Lloyd's Register.
- Forging stock ordered to ASTM A314 for stainless steel billets and bars for forging.
11. Frequently asked questions
What is XM-29 stainless steel?
Is XM-29 the same as Nitronic 33?
What are the minimum mechanical properties of XM-29 bar?
At what temperature is XM-29 forged?
Can XM-29 be hardened by heat treatment?
Is XM-29 magnetic?
Is XM-29 suitable for seawater or subsea service?
Which ASTM specifications cover XM-29?
What information is needed for a quotation?
Request a quotation for XM-29 forgings
Jiangyin Jiangnan Metal Co., Ltd., open die forging factory, Jiangyin, Jiangsu, China. Send a drawing or dimensions and we will quote XM-29 (UNS S24000 / Nitronic 33) rings, flanges, bars, shafts, discs and sleeves.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Related grades
Other nitrogen strengthened and specialty stainless grades we forge: Nitronic 30, Nitronic 32, Nitronic 40, Nitronic 50, Nitronic 60, A182 F51, A182 F53, A182 F55, A182 F44, 904L and A286.
Data sources
Composition, mechanical, thermal and fabrication data on this page are taken from the ASTM A276 and ASTM A240 requirements for XM-29 and UNS S24000, from ASTM A314 for stainless billets and bars for forging, and from published Nitronic 33 and UNS S24000 datasheets. Figures are indicative and do not replace the full specification or the mill certificate for a particular heat. Confirm requirements with our engineering department before ordering.