GRADE X46Cr13 / 1.4034 / AISI 420C   FORM Open-die forged, ring rolled T +86 189 2135 9659   E sales@steelforgepieces.com
Jiangnan Metal Melting works · Open-die forge · Ring mill Get a quote

Home / Stainless Steel / X46Cr13

Martensitic stainless steel / EN 10088-3

X46Cr13 Forgings 1.4034 · AISI 420C · UNS S42000. Bars, rings, sleeves, shafts, discs and pellet mill dies, melted and forged in one works.

X46Cr13 is a hardenable 13 % chromium steel with 0.43 to 0.50 % carbon. It takes a high hardness and a high polish, and it holds up against water, steam and chloride-free media. It is not a seawater grade.

Jiangyin Jiangnan Metal Co., Ltd. melts this steel on site, forges it on a 6,300 t press or rolls it on a 6 m ring mill, heat treats it in one of 14 furnaces and machines it before it ships. The certificate traces back to the melt number, not to a purchased billet.

Grade recordX46Cr13
EN number
1.4034
Standard
EN 10088-3, EN 10088-2
Structure
Martensitic, ferromagnetic
Carbon
0.43 to 0.50 %
Chromium
12.50 to 14.50 %
Max hardness
55 HRC
PREN
12.5 to 14.5
Forging
1180 to 950 °C
Max piece
30,000 kg
Min order
10 kg, no minimum piece count
Lead time
20 to 60 days
01

What X46Cr13 is

X46Cr13 is the European name for a martensitic chromium stainless steel, material number 1.4034, holding 0.43 to 0.50 % carbon and 12.50 to 14.50 % chromium. It is the highest carbon member of the 420 family, which is why it hardens further than the neighbouring grades X39Cr13 (1.4031) and X40Cr14. It is supplied soft annealed for machining at 245 HB maximum, then hardened and tempered in service. Because the structure is martensitic the steel is magnetic.

The trade-off in this grade is carbon against corrosion. Carbon buys hardness and edge retention; it also ties up chromium as carbides. The steel resists water, steam, chloride-free media and some organic acids, and it resists them best when hardened and polished. It does not resist seawater, sulphuric acid or intergranular attack. Where chlorides are in the process stream, a duplex or super austenitic forging is the correct choice and we forge those as well.

02

Equivalent designations

X46Cr13 cross reference
SystemDesignationSystemDesignation
EN number1.4034JISSUS420
EN nameX46Cr13AFNORZ44C14, Z38C13
AISI / SAE420CPN4H13
UNSS42000UNEF.3405
ASTM420GOST40Ch13
BS420S45DIN 17440X46Cr13

Close relatives that are often substituted, and should not be: X39Cr13 (1.4031) and X40Cr14 carry less carbon and reach lower hardness. X46CrS13 (1.4035) adds sulphur for free machining and loses toughness and polishability. Tell us which property drives the part and we will confirm the grade before cutting steel.

03

Chemical composition

X46Cr13 / 1.4034, mass fraction in %, to EN 10088
CSiMnPSCr
0.43 to 0.501.00 max1.00 max0.040 max0.030 max12.50 to 14.50

A narrower carbon band can be agreed at enquiry. Sulphur can be controlled to suit the operation that follows: roughly 0.015 to 0.030 % helps machinability, 0.008 to 0.030 % helps weldability, and 0.015 % maximum is wanted where the part has to take a mirror polish. Elements outside this table are not added deliberately without the buyer agreeing, other than for finishing the cast. Since the heat is melted here, these windows are set in the ladle rather than hunted for on the stock market.

04

Mechanical properties

Soft annealed, +A

Delivery condition for machining
PropertyValue
Tensile strength Rm800 MPa max
Hardness245 HB max
Elongation A12 % min

Published figures run 780 to 800 MPa for this condition. Straightened profiles up to about 35 mm can sit roughly 60 HB and 150 MPa above the annealed values from the cold work alone.

Quenched and tempered, +QT800

Up to 160 mm section
PropertyValue
Tensile strength Rm800 to 1000 MPa
Proof strength Rp0.2650 MPa min
Elongation A5, longitudinal10 % min
Impact energy KV, longitudinal, +20 °C12 J min

Mill datasheets differ on the +QT800 upper tensile limit, with 1000 MPa and 1150 MPa both in print, and on minimum elongation, where 7 % also appears. Above 160 mm diameter the properties are not covered by the table and must be agreed between buyer and supplier. For heavy sections we fix the test position, the test direction and the acceptance values in writing before the heat treatment is booked.

05

Physical properties

X46Cr13 physical data
PropertyValue
Density at 20 °C7.70 kg/dm³
Thermal conductivity at 20 °C30 W/(m·K)
Specific heat capacity at 20 °C460 J/(kg·K)
Electrical resistivity at 20 °C0.55 Ω·mm²/m
Thermal expansion 20 to 100 °C10.5 × 10-6 K-1
Thermal expansion 20 to 200 °C11.0 × 10-6 K-1
Thermal expansion 20 to 300 °C11.5 × 10-6 K-1
Thermal expansion 20 to 400 °C12.0 × 10-6 K-1
MagnetisabilityFerromagnetic
06

Forging and heat treatment

Forging

Heat slowly to above 800 °C, then raise the temperature faster to between 1050 and 1180 °C. Forge on the way down to 950 °C. Some mill datasheets allow finishing as low as 800 °C. After the last blow the piece goes straight into a furnace or into dry ash to cool slowly. At half a percent carbon, air cooling a heavy section off the forging heat is how cracks start, so the cooling step is not optional.

Soft annealing

750 to 850 °C, cooled slowly in the furnace or in air, giving 245 HB maximum. This is the condition we normally ship in when the customer is doing the finish machining.

Hardening and tempering

Austenitise at 950 to 1050 °C, quench rapidly in air or oil, then stress relieve at 200 °C for maximum hardness, which should not run above 55 HRC. Tempering at 650 to 700 °C with air cooling produces the tougher +QT condition. Note the corrosion penalty: high tempering precipitates chromium carbides and leaves depleted zones beside them, so a heavily tempered part corrodes more readily than a hardened and polished one.

Welding

Weldability is very poor and welding is not recommended. If a joint cannot be designed out, preheat to 350 to 400 °C and heat treat afterwards at around 650 °C. Ask us before you order, because a welded assembly usually points to a different grade.

Machining

Machinability is on the poor side and tracks hardness, behaving much like a structural steel at the same hardness. As a starting point with coated carbide on annealed material at 700 to 800 N/mm²: 6 mm depth of cut at 0.5 mm/rev and 115 m/min, 3 mm at 0.4 mm/rev and 140 m/min, 1 mm at 0.2 mm/rev and 160 m/min. Adjust to the actual hardness and the machine.

07

Corrosion behaviour

PREN sits between 12.5 and 14.5, which places X46Cr13 at the low end of the stainless range. Read that number before specifying the grade.

Where the grade holds and where it does not
ConditionBehaviour
Water, steamResistant
Chloride-free media, nitric acidResistant
Hardened and polished surfaceBest corrosion performance of all conditions
Soft annealed or highly temperedReduced, chromium carbides present
Salt, seawaterNot resistant, pitting risk
Sulphuric acidNot resistant
Formic acidMarginal
Intergranular attackNot resistant

Surface finish counts as much as chemistry here. A ground or polished X46Cr13 part outlasts an as-machined one in the same service.

08

What we forge in this grade

Each item is forged from one piece of steel melted on site. No welding, no casting, no bought-in billet of unknown origin.

Bars

Round bars and rods, square, rectangular, flat and hexagonal bars. Black, rough turned, peeled or ground.

Hollow bars and sleeves

Hollow bars, bushes and bushings, cylinders, barrels, casings, shells, hubs and housings, bored from solid forged blanks.

Rings

Seamless rolled rings to 6,000 mm outside diameter on the radial-axial mill, and upset-and-punched forged rings from 50 mm outside diameter.

Shafts, discs, blocks

Shafts, blocks, discs, plates and tube sheets, supplied rough turned or proof machined for volumetric inspection.

Pellet mill dies

Ring die and flat die blanks for feed mills and biomass pellet machines, forged and heat treated to your hardness specification.

Parts to drawing

Any other X46Cr13 forging made to your print, with the heat treatment condition, test position and inspection scope agreed before production.

Works envelope

Limits set by plant equipment
ItemLimitSet by
Heat size60 tEF, LF, VOD route
Single forged piece30,000 kg6,300 t open-die press
Rolled ring diameterup to 6,000 mm OD6 m radial-axial ring mill
Turned lengthup to 14,000 mmC61160 horizontal lathe
Machined diameterup to 5,000 mm5,000 mm vertical lathe
Bored cylinders1,600 mm dia × 10,000 mmCNC deep-hole drilling machine
Heat treatment14 furnacesCar-bottom to 8 m, pit furnaces 15 m deep
ApprovalsCCS, BV, DNV, LR, NKWorks certification
09

Typical uses

Cutting tools and industrial machine knives, knife blades and cutlery, scalpels and surgical instruments, ball and roller bearing components, valves, pumps and pistons, measuring devices, screws, springs and spring wire, carburettor needles, protective sleeves and tubes, and ring dies for feed and biomass pelleting. The grade turns up across mechanical engineering, automotive, food processing, pharmaceutical, bearing and energy work.

10

Questions we get asked

Is X46Cr13 the same as 420 stainless?

It is the high carbon end of the 420 family, AISI 420C. Plain 420 covers a wider carbon band starting lower, so a part specified as 420 may arrive softer than one specified as X46Cr13. If hardness is the point of the part, call out 1.4034 on the drawing.

What hardness can you deliver?

Soft annealed at 245 HB maximum for your own machining, or hardened and tempered to an agreed range up to 55 HRC. State the hardness you want measured, and where on the part you want it measured.

Can you make a ring instead of cutting one from a plate?

Yes, and for this grade it is usually the better route. Ring rolling runs the grain around the circumference instead of cutting through it. We roll to 6,000 mm outside diameter and upset-and-punch smaller rings from 50 mm.

What is the minimum order?

10 kg, with no minimum piece count. One prototype shaft is an acceptable order. Lead time runs 20 to 60 days depending on size, heat treatment and whether a new heat has to be melted.

What documentation comes with the forging?

A mill certificate traceable to the melt number, since the steel is melted in the same works that forges it. Third party inspection by CCS, BV, DNV, LR or NK can be arranged, and we will add ultrasonic testing, magnetic particle inspection, hardness survey or impact testing to the scope on request.

My part sees chlorides. Should I still use this grade?

No. Specify a duplex or super austenitic grade. We forge A182 F51, F53, F44, F61, 904L, Sanicro 28 and the Nitronic range, so changing the grade does not mean changing the supplier.

11

Request a quotation

Send the drawing, or just the grade, shape, finished dimensions and quantity. You get back a price, a forged weight and a lead time. If X46Cr13 is wrong for the duty, we will say so and quote the grade that fits.

CompanyJiangyin Jiangnan Metal Co., Ltd.
Melting works, open-die forge and ring mill, operating since 1997
PlantNo.1 Chengxiqiao Road, Zhouzhuang Town,
Jiangyin City, Jiangsu Province, China
Contact+86 189 2135 9659
sales@steelforgepieces.com

Email the enquiry

12

Other stainless grades

Data on this page is compiled from EN 10088 grade tables and published mill datasheets for 1.4034 and is given for enquiry and design guidance. Binding chemistry, properties, test positions and acceptance criteria are those stated in the order confirmation.