Open-die forging works, Jiangyin, Jiangsu, China. Since 1997. Tel +86 189 2135 9659 Email sales@steelforgepieces.com
Jiangyin Jiangnan Metal Co., Ltd. Melting, open-die forging, ring rolling

Martensitic stainless steel, open-die forging, wear and cutting service

X105CrMo17 Forgings

1.4125 · Z100CD17 · AISI 440C · UNS S44004 · SUS440C · EN 10088-3

X105CrMo17, EN material number 1.4125 and French designation Z100CD17, is a high-carbon martensitic stainless steel with 0.95 to 1.20 percent carbon, 16.0 to 18.0 percent chromium and 0.40 to 0.80 percent molybdenum. Hardened, oil quenched and tempered low, it reaches roughly 58 to 60 HRC, the highest hardness available from a stainless steel. Corrosion resistance is moderate and toughness is low, so the grade is chosen where abrasion and edge holding decide the job and the medium is mild: bearing balls and races, valve seats and seat rings, cutlery and surgical blades, gauge blocks, moulds, dies and pump wear parts.

Jiangyin Jiangnan Metal Co., Ltd. is an open-die forging works in Jiangyin, Jiangsu Province, China. We forge X105CrMo17 into round, flat, square and hexagonal bars, hollow bars, sleeves and bushings, seamless rolled rings, discs, blocks, valve components and bearing race blanks, supplied annealed for machining or hardened and tempered to a stated hardness, with EN 10204 3.1 or 3.2 certification. Each figure below is either a specification limit or a published constant, with the source named against it.

Email an enquiry +86 189 2135 9659

Definition

What is X105CrMo17 / 1.4125?

X105CrMo17 is the EN 10088-3 designation for a high-carbon, high-chromium martensitic stainless steel that is hardened by quenching and low-temperature tempering. The name decodes directly: X marks a high-alloy steel, 105 is the mean carbon content in hundredths of a percent, and CrMo17 gives the main alloying elements with the mean chromium content of 17 percent.

What each element does here:

  • Carbon, 0.95 to 1.20 percent. The reason the grade exists. Part of it dissolves into the martensite and sets matrix hardness; the rest forms hard primary chromium carbides that carry the abrasion resistance and support a cutting edge. It is also why the steel air-hardens and must never be cooled quickly after forging.
  • Chromium, 16.0 to 18.0 percent. High enough that, after a large share is consumed as carbide, the matrix still holds the dissolved chromium needed for a passive film. This is how a steel with one percent carbon can be stainless at all, and why the chromium has to run this high.
  • Molybdenum, 0.40 to 0.80 percent. Improves hardenability so heavier sections harden through, and helps pitting resistance. This is the clearest difference between the EN grade and ASTM 440C, which sets no molybdenum minimum.
  • Manganese and silicon, 1.00 percent maximum each. Deoxidisers and residuals from the melt.
  • Phosphorus 0.040 percent and sulphur 0.030 percent maximum. Residual limits. Sulphur is kept low for hot workability. The free-machining variant 440F runs it high instead, and gives up corrosion resistance for it.
Ordering note. Material ordered to EN 1.4125 satisfies AISI 440C, but the reverse does not hold. ASTM A276 440C and JIS G4303 SUS440C cap molybdenum at 0.75 percent with no minimum, so a 440C heat can contain almost none. If the drawing calls out 1.4125 or Z100CD17, put that on the order rather than accepting 440C equivalent, and the certificate will be issued against the 0.40 to 0.80 percent molybdenum range.

Chemistry

Chemical composition of X105CrMo17 (1.4125)

Table 1. Chemical composition limits, X105CrMo17 / 1.4125 Weight percent to EN 10088-3. Iron is the balance. Product analysis tolerances apply.
ElementMin %Max %Function
Carbon (C)0.951.20Matrix hardness and primary carbide volume
Chromium (Cr)16.0018.00Passivity, carbide former
Molybdenum (Mo)0.400.80Hardenability, pitting resistance
Manganese (Mn)-1.00Deoxidiser, residual
Silicon (Si)-1.00Deoxidiser, residual
Phosphorus (P)-0.040Residual limit
Sulphur (S)-0.030Residual limit, hot workability
Iron (Fe)BalanceBase
Melting at this works runs through an electric arc furnace with ladle refining and vacuum oxygen decarburisation. Electroslag remelting is added where the order calls for tighter carbide distribution and inclusion control, which is worth asking for on bearing races, knife stock and anything that will be mirror polished.

International equivalents

Table 2. X105CrMo17 equivalent grades by standard system Designations used for the same material family, with the chemistry difference noted in the last column.
Region or systemDesignationStandardDifference from 1.4125
Europe (EN)X105CrMo17 / 1.4125EN 10088-3Reference grade
France (AFNOR)Z100CD17NF, superseded by ENNational equivalent
Germany (DIN)W.-Nr. 1.4125DIN 17440 legacySame material number
USA (ASTM / SAE)AISI 440C, UNS S44004ASTM A276, A473Mo 0.75 percent max, no minimum
Japan (JIS)SUS440CJIS G4303Mo capped, no minimum
ISO (bearing steels)X108CrMo17 / 1.3543ISO 683-17Same C, Cr and Mo limits, bearing cleanliness rules
China (GB)108Cr17, cross-referencedGB/T 1220Nearest national designation
Russia (GOST)95Kh18GOST 5632Near only: C 0.90 to 1.00, Cr 17 to 19, no Mo requirement
Related but not interchangeable: X90CrMoV18 / 1.4112 with lower carbon, higher molybdenum and added vanadium, X70CrMo15 / 1.4109 in the 440A class, and X105CrCoMo18-2 / 1.4528 with cobalt. 1.4112 and 1.4125 are often substituted for each other in knife and fitting work, but 1.4125 reaches the higher hardness.

Strength and hardness

Mechanical properties of X105CrMo17

Before quoting tensile figures for this grade. EN 10088-3 lists X105CrMo17 among the martensitic special grades and gives a maximum hardness for the annealed condition, stated for guidance only. It sets no proof strength, tensile strength or elongation minima, because the grade is sold to be machined and then hardened by the user. Tensile numbers circulated for 1.4125 are typical post-heat-treatment values for 440C class material, and Table 4 presents them on that basis. Hardness, not tensile strength, is the acceptance criterion to write into the order.
Table 3. Supply conditions and hardness Annealed limits from ASTM A276 practice for 440C. Hardened values are typical for the class.
Supply conditionHardnessUse
Annealed, hot finished269 HB max, about 29 HRCStandard machining condition
Annealed and cold drawn285 HB max, about 31 HRCBar stock for turned parts
Hardened and tempered low58 to 60 HRC typicalFinal service condition, ground to size
Attainable hardness depends on section size and the exact heat-treatment cycle. Small sections can be air cooled; larger sections are oil quenched for through hardness.

Typical properties after hardening and tempering

The figures below are the published room-temperature values for 440C class material, quenched and then tempered at the temperature shown. They apply to a section of roughly 25 mm, and heavier sections fall below them. Use them for design guidance and confirm hardness on the test piece from your own heat.

Table 4. Typical mechanical properties, hardened and tempered Indicative published values for the 440C / 1.4125 class, about 25 mm section, room temperature. Not specification minima.
ConditionTensile Rm, MPaProof Rp0.2, MPaElongation A50, %HardnessCharpy V, J
Annealed75844814269 HB max-
Hardened, tempered 204 C20301900459 HRC9
Hardened, tempered 260 C19601830457 HRC9
Hardened, tempered 316 C18601740456 HRC9
Hardened, tempered 371 C17901660456 HRC9
Read the elongation and impact columns before selecting the grade: 4 percent elongation and 9 J at full hardness leave almost no ductility reserve. Parts in this steel have to be designed without stress raisers, and shock loading has to be designed out rather than tolerated.

Physical constants

Physical properties of X105CrMo17

Table 5. Physical properties, 1.4125 / 440C Room temperature unless stated. For weight calculation, thermal stress work and machining parameters.
PropertyMetricImperial
Density7.65 g/cm³, 7650 kg/m³0.276 lb/in³
Modulus of elasticity at 20 C200 GPa29 x 10³ ksi
Mean thermal expansion, 0 to 100 C10.1 x 10-6 /K5.6 microin/in per F
Thermal conductivity at 100 C24.2 W/m·K168 Btu·in/ft²·h·F
Specific heat, 0 to 100 C460 J/kg·K0.11 Btu/lb·F
Electrical resistivity0.60 micro-ohm·m, 600 nano-ohm·m361 ohm·cmil/ft
Magnetic responseFerromagnetic in all conditions, annealed and hardened
Usual maximum service temperatureAbout 400 C, limited by the tempering temperature used
Quick weight check: mass in kg is volume in cm³ multiplied by 0.00765. A billet of 300 mm diameter by 200 mm encloses 14,137 cm³ and weighs about 108 kg in this grade. Published constants vary slightly between datasheets, and some European sources give 7.7 g/cm³ and 215 GPa for the 1.4112 and 1.4125 pair. Where a value is critical to the design, state it on the enquiry and it will be confirmed against the datasheet governing the supplied condition.

Thermal processing

Heat treatment and forging of X105CrMo17

Everything useful in this grade is created during heat treatment, and most of what goes wrong with it goes wrong there too. The sequence runs: forge, slow cool, anneal, machine, harden, temper without delay, finish grind.

Table 6. Heat treatment cycles Typical published practice for X105CrMo17 and 440C. Soak until the section is uniform unless stated otherwise.
OperationTemperatureCoolingPurpose and result
Forging1050 to 1150 C, preheat 760 to 820 CSlow, furnace, lime or ashShape and grain flow. Stop forging above 900 C
Annealing840 to 870 C for maximum softnessFurnace coolMachinable condition, 269 HB max
Sub-critical anneal730 to 790 CAir coolSoftening between machining stages
Stress relief, annealed material650 to 760 CSlow coolRemoves machining stress before hardening
Hardening1010 to 1065 CWarm oil quench, small sections air coolMartensite plus undissolved carbides, above 60 HRC as quenched
Tempering150 to 370 C, one hour minimumAir cool58 to 60 HRC, stress relieved
Temper while the part is still hand warm from the quench, and do not leave a hardened part untempered overnight. Tempering above about 400 C is avoided on this grade: corrosion resistance and impact energy both drop and nothing is gained in exchange.

Forging route at this works

  1. Melting and refining Electric arc furnace, ladle furnace and vacuum oxygen decarburisation for carbon and gas control, with electroslag remelting added where the order specifies improved carbide distribution.
  2. Preheat and soak A steel with one percent carbon and 17 percent chromium conducts heat poorly and cracks if it is charged cold into a hot furnace. On heavy sections the preheat stage is not optional.
  3. Forge in the 1050 to 1150 C range Upsetting, drawing and punching on the press line, or ring rolling on radial-axial mills. The finishing passes break up the as-cast carbide network, which is the metallurgical reason to forge this grade rather than cut parts from plate.
  4. Stop above 900 C and reheat Below that temperature the steel loses ductility and tears. Reheats are written into the forging plan rather than decided at the press.
  5. Controlled slow cool, then anneal without delay This grade air-hardens, so finished forgings go to furnace, warm dry lime or ash and are annealed straight away.
  6. Machining in the annealed condition Proof machining for ultrasonic inspection, or rough machining with the allowance the expected heat-treatment distortion requires.
  7. Hardening, tempering and inspection Carried out in instrumented furnaces with recorded charts where the order calls for supply in the hardened condition. Hardness is reported on the same test block as any tensile result.
  8. Certification Chemistry, hardness, mechanical results, heat-treatment charts and NDE reports issued as EN 10204 3.1, or 3.2 endorsed by a third party where required.

Working the material

Machining, welding and corrosion behaviour

Machining

Machine in the fully annealed condition. The carbon content makes it behave somewhat like a high-speed steel, with tough stringy chips, so chip breakers matter. Once hardened it becomes a grinding job. Where a part needs heavy machining and 60 HRC is not required, the free-machining 440F variant is the usual alternative.

Welding

Rarely welded, and better designed out. The heat-affected zone air-hardens and cracks. If welding cannot be avoided, preheat, use a suitable austenitic or matching consumable, then anneal and furnace cool. A one-piece forging removes the problem, which is why valve seats and sleeves in this grade are forged rather than fabricated.

Corrosion resistance

Moderate, and below the 300-series austenitic grades, because a large share of the chromium sits in carbides rather than in solution. Acceptable in fresh water, mild domestic and industrial atmospheres, food, organic media and many petroleum products. Not for strong acids, chlorides or chlorine.

Surface finish

Corrosion performance on this grade depends heavily on the surface. A smooth, burr-free, polished surface passivates reliably, while a rough or scaled one will pit in service that a polished part survives. Specify the finish on the order rather than relying on the grade alone.

Temperature limits

Service is held to roughly 400 C, and in practice below the tempering temperature used. The grade is also not recommended for sub-zero duty, where the low impact energy becomes the governing problem.

Retained austenite

High-carbon stainless grades retain austenite after quenching, which can cause dimensional drift in precision parts. For gauge blocks, bearing races and measuring instruments, specify sub-zero treatment and double tempering on the order.

Capability

X105CrMo17 forgings we produce

All items are forged from a single piece of steel to customer drawing or to a standard dimensional specification, and supplied as forged, annealed, rough machined or finish machined.

Table 7. Forged product forms in X105CrMo17 / 1.4125 / Z100CD17
Forged formTypical componentsDimensional basis
Forged barsRound bars, rods, square, rectangular, flat and hexagonal bars, knife and machining stockDiameter or section by length
Hollow bars and sleevesBushes, bushings, pipes, tubes, barrels, casings, shells, cylinders, hubs, housingsOD by ID by length
Seamless rolled ringsBearing races, valve seat rings, retaining rings, wear ringsTo drawing
Forged ringsSections outside the ring mill envelope, upset and punchedTo drawing
Discs, blocks and platesDie blocks, mould blocks, gauge blocks, blanks, closuresTo drawing
Valve componentsValve seats, seat rings, stems, bodies, bonnets, nozzles, plugsTo drawing
Bearing and wear partsBall bearing races, rollers, pivot pins, guide rollers, textile wear partsTo drawing
Cutting and instrument blanksKnife and cutlery blanks, surgical instrument blanks, measuring instrument partsTo drawing

Where the grade is used

Table 8. Applications and the property that drives the selection
IndustryComponentsWhy this grade
BearingsBall bearings, races, rollers, bushingsHighest hardness available from a stainless steel, with corrosion resistance a through-hardening bearing steel cannot offer
Valves and flow controlSeats, seat rings, stems, bodies, bonnets, nozzles, plugsGalling and erosion resistance at sealing faces in mild media
Cutlery and bladesKnife blades, food processing knives, surgical bladesEdge retention at 58 to 60 HRC with food-contact corrosion resistance
ToolingMoulds, dies, die blocks, plastic moulding toolingTakes a high polish and resists wear in tooling exposed to condensate
MetrologyGauge blocks, measuring instruments, precision fixturesDimensional stability after correct heat treatment, hard wearing faces
Pumps and processPump wear parts, sleeves, pivot pins, plungersAbrasion resistance in mild aqueous and petroleum service
Textile machineryGuide rollers, wear components, cutting elementsContinuous abrasive contact without lubrication

Selection

X105CrMo17 compared with neighbouring martensitic grades

Table 9. Choosing between the high-carbon martensitic stainless grades Composition limits as published for each grade. Hardness is typical attainable, not a specification value.
GradeNumberC %Cr %Mo %Choose it when
X105CrMo171.41250.95 to 1.2016 to 180.40 to 0.80Hardness and wear resistance decide the job, 58 to 60 HRC
X90CrMoV181.41120.85 to 0.9517 to 190.90 to 1.30More corrosion margin and a little more toughness are worth giving up a few HRC. Vanadium 0.07 to 0.12
X70CrMo151.41090.60 to 0.7514 to 160.40 to 0.80Toughness and formability matter more than peak hardness, 440A class
X105CrCoMo18-21.45281.00 to 1.1016.5 to 18.51.00 to 1.50Hot hardness beyond what 1.4125 holds. Cobalt 1.3 to 1.8
AISI 440AS440020.60 to 0.7516 to 180.75 maxLowest carbon of the 440 family, best corrosion resistance in the group
GOST 95Kh18-0.90 to 1.0017 to 190.20 maxOnly where a Russian specification is mandated. No molybdenum requirement
How selection usually runs on these enquiries: start at 1.4125 when wear governs and the medium is mild, move to 1.4112 where the part sees slightly more aggressive media, and move out of the 440 family entirely, to duplex, 17-4PH or a nickel alloy, as soon as chlorides, acids or sub-zero toughness enter the specification.

Specifications

Standards covering X105CrMo17 and its equivalents

Table 10. Specifications commonly invoked on orders for this grade
ReferenceScope and how it applies
EN 10088-3Stainless steel semi-finished products, bars, rods, sections and wire for general purposes. The governing standard for X105CrMo17 / 1.4125 and the source of the composition limits in Table 1.
ASTM A276Stainless steel bars and shapes, covering 440C / UNS S44004 and the annealed hardness limits in Table 3.
ASTM A473Stainless steel forgings. The usual US reference when the grade is ordered as a forging rather than as bar.
ISO 683-17Ball and roller bearing steels, which list the grade as X108CrMo17 / 1.3543 with bearing cleanliness requirements.
JIS G4303Stainless steel bars, SUS440C.
GB/T 1220Chinese stainless steel bar standard, nearest designation 108Cr17.
EN 10204Inspection documents. 3.1 is issued by the works, 3.2 is counter-endorsed by a third party.
EN 10228-3 and ASTM A388Ultrasonic examination procedures and acceptance classes applied to forgings in this grade.

Ordering

Request a quotation for X105CrMo17 forgings

Send a drawing, or the six items below, and the enquiry can be priced without a second round of questions.

Table 11. What to include in the enquiry
#ItemExample
1Grade and standardX105CrMo17 / 1.4125 to EN 10088-3, or 440C to ASTM A473
2Form, dimensions or drawingRing OD 620 by ID 480 by H 95 mm, or bar 120 mm diameter by 2000 mm
3Quantity and repeat volume24 pieces, about three batches a year
4Delivery conditionAnnealed to 269 HB max, or hardened and tempered to 58 to 60 HRC
5Testing and NDEHardness, chemistry, ultrasonic to EN 10228-3, sub-zero treatment where dimensional stability is critical
6Certification and destinationEN 10204 3.1, or 3.2 witnessed by a nominated agency, and the port of discharge

Email sales@steelforgepieces.com Call +86 189 2135 9659

Jiangyin Jiangnan Metal Co., Ltd.
Open-die forging works, No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Operating since 1997. Melting, open-die forging, ring rolling, heat treatment, machining and testing on one site.

Telephone +86 189 2135 9659. Email sales@steelforgepieces.com.

Prepared by the technical department. Published 9 October 2026, last reviewed 9 October 2026. Composition limits from EN 10088-3. Annealed hardness limits from ASTM A276 practice for 440C. Heat-treated mechanical and physical values are published datasheet figures for the 440C and 1.4125 class. Equivalent designations cross-referenced against EN, ASTM, JIS, ISO 683-17, GB/T 1220 and GOST 5632.

Questions

Frequently asked questions about X105CrMo17

What is X105CrMo17 steel?

X105CrMo17 is a high-carbon martensitic stainless steel to EN 10088-3, material number 1.4125, containing 0.95 to 1.20 percent carbon, 16.0 to 18.0 percent chromium and 0.40 to 0.80 percent molybdenum. The high carbon forms chromium carbides that give high hardness and wear resistance after hardening and tempering, typically 58 to 60 HRC, with lower corrosion resistance and toughness than lower-carbon stainless grades.

Is X105CrMo17 the same as 440C?

They are the same material family and are normally supplied against each other. EN X105CrMo17 / 1.4125, French Z100CD17, AISI 440C / UNS S44004 and JIS SUS440C all specify 0.95 to 1.20 percent carbon and 16.0 to 18.0 percent chromium. The difference is molybdenum: EN 1.4125 requires 0.40 to 0.80 percent, while ASTM 440C and JIS SUS440C set a maximum of 0.75 percent with no minimum. Material ordered as 1.4125 therefore meets 440C, but 440C does not automatically meet 1.4125.

What hardness can X105CrMo17 reach?

About 58 to 60 HRC after hardening, oil quenching and low-temperature tempering, depending on section size and the exact cycle. In the annealed condition ASTM A276 limits the grade to 269 HB maximum as hot finished, or 285 HB maximum annealed and cold drawn, which is the condition in which it is machined before final heat treatment.

Does EN 10088-3 give tensile minima for 1.4125?

No. EN 10088-3 lists X105CrMo17 among the martensitic special grades with a maximum hardness in the annealed condition, stated for guidance only, and no proof strength, tensile strength or elongation minima. The grade is bought to be machined and then hardened by the user, so hardness is the correct acceptance criterion. Tensile figures published for this steel, including the familiar 758 MPa annealed and 2030 MPa hardened values, are typical heat-treated data for the 440C class rather than specification minima.

How is X105CrMo17 forged?

Preheat slowly, raise uniformly to the forging range of about 1050 to 1150 C, soak until the section is uniform and forge without delay, stopping before the steel falls below about 900 C. The grade air-hardens, so finished forgings are cooled slowly in a furnace, in warm dry lime or in ash, then annealed immediately. Cooling a forging of this grade in still air can crack it.

How corrosion resistant is X105CrMo17?

Moderate. Much of the chromium is tied up as carbide rather than dissolved in the matrix, so resistance sits below that of the 300-series austenitic stainless steels. It performs acceptably in fresh water, mild domestic and industrial atmospheres, organic media, food and many petroleum products, and it is not suitable for strong acids or chloride-bearing service. Resistance is highest in the hardened and tempered condition with a smooth polished surface.

Can X105CrMo17 be welded?

It is rarely welded, because the high carbon content makes the heat-affected zone air-harden and crack. Where welding cannot be avoided, preheat, use a suitable austenitic or matching consumable, then anneal and furnace cool. Making the part as a one-piece forging removes the heat-affected zone altogether, which is the usual route for valve seats, bearing races and sleeves in this grade.

Why forge this grade instead of machining it from plate or bar?

Two reasons. Grain flow stays continuous around the part contour, which a ring cut from plate cannot reproduce. More importantly for this particular steel, a one percent carbon stainless solidifies with a coarse primary carbide network, and the hot work of forging is what breaks that network down. Carbide size and distribution decide whether a bearing race or a polished mould surface performs, so the forging reduction is doing metallurgical work and not just producing a shape.

What forms are available in X105CrMo17?

Forged round, square, flat and hexagonal bars; hollow bars, sleeves, bushings, cylinders, casings, shells, hubs and housings; seamless rolled rings and forged rings; discs, blocks and plates; bearing races, valve seats, valve stems, seat rings, bodies, bonnets, nozzles, pivot pins, gauge blocks, die and mould blanks, knife blanks and surgical instrument blanks. Parts are supplied as forged, annealed, rough machined or finish machined.

Who supplies X105CrMo17 forgings from China?

Jiangyin Jiangnan Metal Co., Ltd., a steel melting and open-die forging works at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, operating since 1997. The works melts its own steel, forges and ring rolls, heat treats and machines on one site, and certifies to EN 10204 3.1 or 3.2. Enquiries: sales@steelforgepieces.com, +86 189 2135 9659.