1.4854 forgings — X6NiCrSiNCe35-25 / UNS S35315
Heat-resisting austenitic rings, flanges, discs, tube sheets, shafts, sleeves, bushings and bar, forged to drawing from steel melted at our own works in Jiangyin, Jiangsu, China.
1.4854 is the EN material number for X6NiCrSiNCe35-25, an austenitic heat-resisting steel of about 25 % chromium and 35 % nickel, alloyed with nitrogen and carrying a cerium addition of 0.03 to 0.08 %. Its UNS number is S35315. It is specified in EN 10095, the European standard for heat resisting steels and nickel alloys, which flags it as a patented steel grade.
The grade belongs in furnaces, not in seawater. EN 10095 allows it up to 1170 °C in air. Metalcor credits it with good creep rupture strength, very good high-temperature corrosion resistance and scaling resistance to 1100 °C, and gives heat treatment furnaces as the application. Alleima attributes the oxidation resistance to the silicon content together with the rare earth addition, which also keeps the oxide scale attached through temperature cycling.
We forge it to order. Minimum 10 kg with no minimum piece count, single pieces to 30 tonnes, rolled rings to 6,000 mm outside diameter, EN 10204 3.1 certification as standard and 3.2 witnessed on request.
Designations and standards
| System | Designation |
|---|---|
| EN material number | 1.4854 |
| EN steel name | X6NiCrSiNCe35-25 |
| UNS | S35315 |
| Common trade name | 353 MA. Alleima records this as a trademark owned by Outokumpu OY, so it is used here only to identify the grade. |
| Material standard | EN 10095, covering semi-finished products, sheet, plate, strip, bars, rods and sections in heat resisting steels and nickel alloys |
| Tube product standards quoted by Alleima | ASTM A312, EN 10297-2 |
Forgings in this grade are normally ordered to EN 10095 chemistry and heat treatment, with dimensions, testing and acceptance written into the purchase specification or the drawing. Tell us which standard your inspection body will read from and we will write the certificate against it.
Chemical composition
The specification range below is the EN 10095 cast analysis. Mills aim at a nominal point inside it, which is why a mill certificate carries single figures rather than ranges.
| Element | EN 10095 range | Alleima nominal |
|---|---|---|
| Carbon, C | 0.04 to 0.08 | 0.07 |
| Silicon, Si | 1.20 to 2.00 | 1.6 |
| Manganese, Mn | 2.00 max | 1.5 |
| Phosphorus, P | 0.040 max | 0.040 max |
| Sulphur, S | 0.015 max | 0.015 max |
| Chromium, Cr | 24.00 to 26.00 | 25 |
| Nickel, Ni | 34.00 to 36.00 | 35 |
| Nitrogen, N | 0.12 to 0.20 | 0.16 |
| Cerium, Ce | 0.03 to 0.08 | 0.05 |
Alleima adds that other rare earth metals should be counted with the cerium, since the addition is made as misch metal containing about 50 % cerium. Metalcor works to a tighter silicon limit of 1.30 % max and nitrogen 0.17 % max on its own supply, so confirm which acceptance range applies before the heat is poured.
Mechanical properties at 20 °C
| Property | EN 10095 | Alleima, seamless tube |
|---|---|---|
| Proof strength Rp0.2 | 300 N/mm² min | 300 MPa min (44 ksi) |
| Proof strength Rp1.0 | 340 N/mm² min | 340 MPa min (49 ksi) |
| Tensile strength Rm | 650 to 850 N/mm² | 650 MPa min (94 ksi) |
| Elongation A | 40 % min | 40 % min, A2" 35 % min |
| Hardness | 210 HB max | about 160 HV |
| Modulus of elasticity | not specified | 190 GPa |
EN 10095 lists these values for flat products to 75 mm, bars to 160 mm and rods to 25 mm in the +AT condition. For rods only the tensile strength applies. For sections and bars of 35 mm and under with a final cold deformation, the standard permits hardness 100 units higher or tensile strength 200 N/mm² higher, with elongation down to 20 %. Metalcor quotes Rm 650 to 800 N/mm² and hardness 152 HB 30 max for its material.
Strength at temperature
| Temperature, °C | Rp0.2, MPa | Rp1.0, MPa | Rm, MPa |
|---|---|---|---|
| 100 | 228 | 261 | 536 |
| 200 | 195 | 223 | 498 |
| 300 | 166 | 190 | 470 |
| 400 | 152 | 173 | 444 |
| 500 | 143 | 163 | 437 |
| 600 | 138 | 159 | 422 |
Creep strength
Above roughly 550 °C the design limit is creep rather than proof strength. EN 10095 and the Alleima datasheet publish the same average values where they overlap, which is a useful cross-check.
| Temperature, °C | 1 % in 10,000 h | 1 % in 100,000 h | Rupture in 10,000 h | Rupture in 100,000 h |
|---|---|---|---|---|
| 600 | 88 | 52 | 127 | 80 |
| 700 | 35 | 21 | 56 | 36 |
| 800 | 15 | 9.7 | 28 | 18 |
| 900 | 8 | 5.1 | 15 | 9.2 |
| 1000 | 4.5 | 3.0 | 8 | 4.8 |
| 1100 | 2.7 | 1.8 | 4.5 | 2.9 |
Values to 1000 °C follow the EN 10095 creep tables for the +AT condition; the 1100 °C row and the intermediate 50 °C steps come from the Alleima datasheet. These are estimated average values for comparison between grades, not design allowables for a specific forging.
Physical properties
| Property | At 20 °C | At temperature |
|---|---|---|
| Density | 7.9 g/cm³ | – |
| Thermal conductivity | 11 W/m °C | 20 at 500 °C, 27 at 1000 °C |
| Specific heat capacity | 480 J/kg °C | 590 at 500 °C, 665 at 1000 °C |
| Mean thermal expansion | 15.5 × 10-6 /°C, 20 to 100 °C | 18 × 10-6 /°C, 20 to 1000 °C |
| Modulus of elasticity | 190 GPa | 155 GPa at 600 °C, 130 GPa at 1000 °C |
| Electrical resistivity | 1.00 µΩ·m | 1.30 µΩ·m at 1000 °C |
Why the grade behaves the way it does
Oxidation
Alleima puts the high oxidation resistance down to the silicon content plus the rare earth metal addition, which also improves how well the scale stays attached during thermal cycling. Scale spalling under cycling is what shortens the life of plain 310-type steels in batch furnaces.
Carburisation
The dense chromium oxide and the 35 % nickel give good resistance to carburisation and nitrogen pick-up. Alleima's rate-constant data shows the grade holding up under cyclic carburising and oxidising conditions better than the alloys it was tested against.
Nitriding
In nitrogen pick-up tests in cracked ammonia, Alleima reports resistance similar to Alloy 601. That is why the grade turns up in ammonia dissociator hardware and bright annealing lines.
Sulphur
High-nickel alloys are generally sensitive to sulphur attack at temperature. Alleima notes that under oxidising conditions a protective oxide forms and improves the picture. Sulphidising service should be stated at enquiry rather than assumed.
Service temperature
EN 10095 gives a maximum application temperature in air of 1170 °C, defined on the basis that scaling loss does not exceed 1 g/m²h at that temperature. Metalcor states scaling resistance to 1100 °C. Alleima gives approximately 1175 °C as the maximum operating temperature for its tube and publishes oxidation data measured at 1150 °C. The three figures are consistent once the basis is read: they describe scaling, not load-carrying ability. The creep table above is what limits a loaded component, and it falls away quickly above 800 °C.
Heat treatment, welding and forming
| Operation | Recommendation |
|---|---|
| Solution annealing | 1100 to 1150 °C with sufficiently rapid cooling in water or air, per EN 10095 condition +AT. Alleima gives 1100 to 1200 °C for 5 to 20 minutes, rapid cooling in air or water. Soak time on a heavy forging is set by section thickness. |
| Stress relieving | 1000 to 1100 °C for 10 to 15 minutes, cooled in air (Alleima). |
| Welding process | Weldability is good. TIG/GTAW is the first choice, with MIG/GMAW and MMA/SMAW also suitable. |
| Filler metals | ISO 18274 S Ni 6082 / AWS A5.14 ERNiCr-3 for TIG and MIG; ISO 14172 E Ni 6182 / AWS A5.11 ENiCrFe-3 for MMA. Metalcor also lists 1.4854 itself as a suitable matching filler, so check what your fabrication code allows. |
| Welding parameters | Heat input under 1.0 kJ/mm, interpass temperature under 100 °C. Low thermal conductivity and high expansion mean the weld sequence should be planned for distortion. Solution annealing after welding is an option where residual stress matters. |
| Cold bending | Higher deformation forces are needed than for conventional stainless steels. Annealing after cold bending is not normally required, but the decision should account for the degree of bending and the service conditions. |
Where the grade is used
This is a furnace and hot-gas grade. The published application list, driven by the combination of oxidation, carburisation and nitriding resistance, is as follows.
| Service | Components |
|---|---|
| Petrochemical furnaces | Ethylene furnace radiant cracking tubes; EDC furnace tubes |
| Metallurgical waste heat recovery | Recuperator tubes |
| Heat treatment furnaces | Muffle tubes, radiant tubes, thermocouple protection tubes, burner components, furnace rollers |
| Incineration | Recuperator tubes in chemical waste and sewage sludge incineration |
Translated into forged shapes, the parts we are most often asked to price in this grade are furnace roller journals, hubs and end caps, radiant tube and retort flanges, recuperator tube sheets and covers, burner nozzles and sleeves, rolled rings for furnace and kiln hardware, fan and rotor hubs for hot gas circulation, and bar for machined furnace fixtures. Those are component families from our own order book rather than published data, so suitability for a particular part still has to be checked against your operating temperature, load and atmosphere.
A word on grade selection. 1.4854 is sometimes listed alongside seawater and acid alloys. It does not belong there. For chloride-bearing seawater, subsea and sour service the relevant grades are super duplex A182 F55 and A182 F53, duplex A182 F51, or super austenitic A182 F44 and 904L. If a part has to take heat and wet corrosion together, send both conditions and we will select against whichever governs.
Forged products in 1.4854
Seamless rolled rings
Radial-axial rolled from a punched preform, rectangular or contoured section, to 6,000 mm outside diameter on the 6 m mill, with 3 m and 1 m mills for smaller sizes.
Forged rings
Upset and punched rings from OD 50 mm, for sections outside the ring mill envelope and where heavy reduction is preferred to rolling.
Forged flanges
Weld neck, blind, slip-on, lap joint, orifice and long weld neck patterns, plus non-standard furnace and retort flanges to drawing.
Discs and tube sheets
Solid forged discs, recuperator and exchanger tube sheets and covers, supplied proof-machined where volumetric inspection is required.
Shafts and rolls
Furnace roller shafts, stepped shafts and spindles. Two 15 m well-type furnaces allow long shafts to be quenched vertically.
Cylinders, sleeves, bushings
Hollow forged cylinders and heavy-wall sections bored from solid, to 1,600 × 10,000 mm on the CNC deep-hole drilling machine.
Bar and blocks
Round, flat and square forged bar as feedstock for machined furnace fixtures and hot-zone hardware.
Machined components
Bodies, blocks, nozzles, seat rings and sleeves, supplied as-forged, proof-machined or finish-machined to drawing.
How we make it
We melt our own steel rather than buying billet, which counts for more than usual on a nitrogen and cerium alloyed grade: the analysis is aimed at the forging it will become, and the certificate goes back to a melt number instead of stopping at a purchased billet.
| Step | Equipment |
|---|---|
| Melting and refining | 25 t electric arc furnace; 25 t and 50 t ladle furnaces; 30 t and 60 t vacuum oxygen decarburisation, used where nitrogen has to be held inside a narrow band. Maximum heat size 60 t. |
| Remelting where specified | 3 t and 6 t protective-atmosphere electroslag remelting; 3 t vacuum induction melting and 6 t vacuum arc remelting for superalloy work. |
| Forging | 6,300 t, 4,000 t and 2,000 t hydraulic open-die presses; 5 t, 3 t, 2 t, 1 t and 750 kg hammers. Heaviest single forging 30 t. |
| Ring rolling | Radial-axial mills at 6 m, 3 m and 1 m maximum outside diameter. |
| Heat treatment | 14 furnaces, including three high-temperature car-bottom furnaces RTX-12-350KW with a 3,500 × 1,300 × 1,100 mm chamber covering the solution treatment range this grade needs, and two 15 m well-type furnaces for vertical quenching of long shafts. |
| Machining | Vertical lathes to 5,000 mm swing, horizontal lathes to 14 m between centres, CNC machining and deep-hole drilling to 1,600 × 10,000 mm. |
Testing and certification
Each forging is released against a documented route: melt analysis, mechanical testing on a representative test piece, non-destructive examination, dimensional inspection, then certification.
| Test | Equipment or route | Standard |
|---|---|---|
| Chemical analysis | Optical emission spectrometer SPECTROTEST TXC25 | ASTM E415 |
| Carbon and sulphur | Infrared analyser HIR-9440D | ASTM E1019 |
| Alloy verification | Handheld analyser X-Mwt3000TX | Positive material identification |
| Tensile | 600 kN WE-600B and WDW-300 | ASTM A370, ISO 6892 |
| Impact | JBN-300 with DWC-60 low-temperature bath | ASTM A370 |
| Ultrasonic | PXUT-3300, USM35XS, CTS-22 | ASTM A388, EN 10228-3 |
| Magnetic particle | CYE-3A | ASTM E709 |
| Grain size and metallography | XJP-6A microscope with specimen preparation | ASTM E112 |
| Intergranular corrosion, when specified | Placed with an accredited third-party laboratory, report issued with the mill certificate | ASTM A262, ASTM G28 |
Certification is EN 10204 3.1 as standard and EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector on request. The works holds CCS, BV, DNV, LR and NK approvals.
Ordering
| Item | Detail |
|---|---|
| Supply basis | Made to order from a drawing or specification. Manufacturer, not a stockist or trading company. |
| Minimum order | 10 kg, no minimum piece count |
| Quotation | Within 2 working days of a complete enquiry |
| Lead time | 20 to 60 days by material route and testing scope |
| Delivery condition | As-forged, proof-machined or finish-machined |
| Drawing formats | PDF, DWG, DXF, STEP |
Request a price for 1.4854 forgings
Send the grade, the dimensions or a drawing, the quantity, the delivery condition, the heat treatment and testing scope, and the destination. Those six items are what an estimator needs to price the job without going back and forth.
Email sales@steelforgepieces.com +86 189 2135 9659 Contact page
Jiangyin Jiangnan Metal Co., Ltd. · No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China 214423 · Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8) · English and Chinese.
Frequently asked questions
What is 1.4854 steel?
1.4854 is the EN material number for X6NiCrSiNCe35-25, an austenitic heat-resisting chromium-nickel steel of about 25 % Cr and 35 % Ni, alloyed with nitrogen and with 0.03 to 0.08 % cerium. Its UNS number is S35315 and it sits in EN 10095, which marks it as a patented steel grade.
What is the chemical composition of 1.4854?
To EN 10095: C 0.04 to 0.08, Si 1.20 to 2.00, Mn 2.00 max, P 0.040 max, S 0.015 max, Cr 24.00 to 26.00, Ni 34.00 to 36.00, N 0.12 to 0.20, Ce 0.03 to 0.08, balance iron. Alleima's nominal analysis inside that envelope is 0.07 C, 1.6 Si, 1.5 Mn, 25 Cr, 35 Ni, 0.16 N, 0.05 Ce.
What are the mechanical properties of 1.4854?
EN 10095 requires Rp0.2 300 N/mm² min, Rp1.0 340 N/mm² min, Rm 650 to 850 N/mm², elongation 40 % min and hardness 210 HB max. Alleima quotes the same minima for solution-annealed tube with hardness around 160 HV. Modulus of elasticity at 20 °C is 190 GPa.
What is the maximum service temperature?
EN 10095 gives 1170 °C as the maximum application temperature in air. Metalcor states scaling resistance to 1100 °C and Alleima gives approximately 1175 °C for its tube. Under load the limit is creep: average 100,000 h rupture strength is 36 MPa at 700 °C, 18 MPa at 800 °C, 9.2 MPa at 900 °C and 4.8 MPa at 1000 °C.
What is 1.4854 used for?
Ethylene furnace radiant cracking tubes, EDC furnace tubes, recuperator tubes in metallurgical waste heat recovery, heat treatment furnace hardware including muffle tubes, radiant tubes, thermocouple protection tubes, burner components and furnace rollers, and recuperator tubes in chemical waste and sewage sludge incineration.
Is 1.4854 suitable for seawater or acid service?
No. It is a heat-resisting grade for oxidising, carburising and nitriding atmospheres at high temperature. Seawater, sour and strong acid duty calls for duplex, super duplex or super austenitic grades instead.
How is 1.4854 heat treated after forging?
EN 10095 specifies solution annealing at 1100 to 1150 °C with sufficiently rapid cooling in water or air. Alleima gives 1100 to 1200 °C for 5 to 20 minutes, and stress relieving at 1000 to 1100 °C for 10 to 15 minutes cooled in air. Section thickness sets the soak time. Our three high-temperature car-bottom furnaces cover this range on site.
Which filler metal is used to weld 1.4854?
ISO 18274 S Ni 6082 or AWS A5.14 ERNiCr-3 for TIG and MIG, and ISO 14172 E Ni 6182 or AWS A5.11 ENiCrFe-3 for MMA, with heat input below 1.0 kJ/mm and interpass temperature below 100 °C. Metalcor also lists 1.4854 as a matching filler, so check your fabrication code.
How large a ring can you roll in this grade?
Seamless rings roll to 6,000 mm outside diameter on the 6 m radial-axial mill, with 3 m and 1 m mills for smaller sizes and an upset-and-punch route from OD 50 mm. The heaviest single forging of any type is 30 tonnes.
What is the minimum order and lead time?
Minimum order is 10 kg with no minimum piece count. Lead time is 20 to 60 days depending on the material route and the testing scope, and a quotation comes back within two working days of a complete enquiry.
Related grades
Grades commonly compared with or specified alongside 1.4854 for high-temperature work: AISI 330, Incoloy 800H, Incoloy 800HT, Inconel 601, Inconel 600, Inconel 617, Haynes 230 and Alloy 602. Full listings: stainless steel grades and nickel alloy grades.
Reference data
Composition, mechanical limits, heat treatment, maximum application temperature and creep values are taken from EN 10095. Nominal analysis, physical properties, welding and forming data are taken from the Alleima 353 MA seamless tube datasheet. Scaling resistance and supplementary hardness data are taken from the Metalcor datasheet for 1.4854. Published third-party data is reproduced here for grade selection; the figures that govern an order are those on the mill certificate issued with the parts.
Page last reviewed 26 September 2026.