Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory, Jiangyin, Jiangsu, China Call +86 189 2135 9659 Email sales@steelforgepieces.com
Jiangyin Jiangnan Metal Co., Ltd. Open-die forgings, seamless rolled rings and forged bars

20NiCrMoS6-4 case hardening steel forgings EN material number 1.6571. EN 10084:2008. Alloy carburising steel.

20NiCrMoS6-4 is a nickel chromium molybdenum case hardening steel listed in EN 10084 under the material number 1.6571. The letter S means sulphur is added on purpose, 0.020 to 0.040 per cent, to make the steel easier to machine. After carburising, quenching and a low temper the surface reaches about 58 to 62 HRC while the core stays tough, which is why the grade is normally picked for gears, pinions and transmission shafts. Jiangyin Jiangnan Metal Co., Ltd. is an open-die forging factory in Jiangyin, Jiangsu, China. We forge 20NiCrMoS6-4 to customer drawing as rings, shafts, gear blanks, discs, flanges and bars, and supply it with an EN 10204 3.1 or 3.2 certificate.

EN material number
1.6571
Standard
EN 10084:2008
Steel group
Case hardening
Typical case hardness
58–62 HRC
Core Rm, d ≤ 16 mm
≥ 1200 N/mm²
Soft annealed (+A)
≤ 229 HBW
Send a drawing for a quote +86 189 2135 9659 Send a drawing or the finished dimensions and we will price it.

What 20NiCrMoS6-4 is, and when to use it

20NiCrMoS6-4 sits in the group of alloy case hardening steels covered by EN 10084. These steels keep carbon low so that the core stays tough, and they carry nickel, chromium and molybdenum so that a carburised skin hardens right through when the part is quenched. Inside the 1.6566 / 1.6569 / 1.6571 family this is the version with more carbon and with sulphur added. The same grade also appears in EN 10263-3, which covers bar and wire for cold heading.

The name can be read straight off. 20 is the nominal carbon content in hundredths of a per cent, so about 0.20 per cent C. NiCrMo lists the alloying elements in order of content. S flags the sulphur addition. 6-4 gives nickel and chromium divided by four, so nominally 1.5 per cent Ni and 1.0 per cent Cr.

This grade suits the job when

  • the part is carburised and needs a hard, wear resistant skin over a core that can take shock, such as gear teeth, splines, races and pins;
  • there is a lot of machining to do, and free cutting behaviour saves more money than the last few joules of transverse toughness are worth;
  • sections are medium to heavy, so the nickel is needed to harden the core through;
  • a European specification is called up and 1.6571 is written on the drawing.

Look at another grade when

  • transverse toughness and ultrasonic cleanliness govern. Use 17NiCrMo6-4 (1.6566), which has no sulphur addition.
  • sections are very heavy and you need deeper hardenability. Use 18CrNiMo7-6 (1.6587).
  • the part is through hardened rather than carburised. Use a quenched and tempered grade such as 42CrMo4 or 34CrNiMo6.
  • the part holds pressure. A carburising steel is the wrong family. Ask us about the carbon steel and stainless pressure grades instead.

Chemical composition of 20NiCrMoS6-4 (1.6571)

Composition limits for 20NiCrMoS6-4 as given in EN 10084:2008, mass per cent, balance iron.

Table 1. Chemical composition of 20NiCrMoS6-4 / EN 1.6571, mass %, to EN 10084:2008.
ElementMinMaxWhat it does here
Carbon, C0.160.23Sets core strength, low enough to keep the core tough
Silicon, Si–0.40Deoxidiser
Manganese, Mn0.500.90Hardenability, and binds sulphur as MnS
Phosphorus, P–0.025Residual, kept low for toughness
Sulphur, S0.0200.040Added on purpose, breaks chips, free machining
Chromium, Cr0.600.90Case hardenability and wear resistance
Molybdenum, Mo0.250.35Hardenability, resists temper embrittlement
Nickel, Ni1.401.70Core toughness, in particular at low temperature
Iron, FeBalance–
Published sources do not fully agree. Mill datasheets that put 1.6566, 1.6569 and 1.6571 on one page, such as the Saarstahl sheet, quote one typical analysis for the whole family with different bands: Cr 0.80 to 1.10 per cent, Ni 1.20 to 1.50 per cent, Mo 0.15 to 0.25 per cent. Both versions circulate online. Work to the limits in the edition of EN 10084 named on your drawing, and accept material against the ladle analysis printed on the EN 10204 certificate for the heat you are actually supplied. We send you the analysis of each heat before forging starts.

Mechanical and physical properties

Hardness as delivered

Case hardening steels are delivered soft so the customer can machine them, then carburised and hardened afterwards. EN 10084 sets out the delivery conditions below.

Table 2. Hardness of 20NiCrMoS6-4 in each EN 10084 delivery condition.
SymbolDelivery conditionBrinell hardness
+STreated for shearability≤ 255 HBW
+ASoft annealed≤ 229 HBW
+THTreated to a hardness range179–229 HBW
+FPTreated to a ferrite pearlite structure and hardness range154–207 HBW

Soft annealed, the tensile strength runs about 590 to 730 N/mm² with a reduction of area near 55 to 60 per cent.

Core properties after case hardening

These figures come from test pieces carburised, hardened and tempered at 200 °C. They describe the core, not the hardened case.

Table 3. Minimum core tensile strength of 20NiCrMoS6-4 after hardening and tempering at 200 °C.
Ruling section, dTensile strength Rm
d ≤ 16 mm≥ 1200 N/mm²
16 mm < d ≤ 40 mm≥ 1000 N/mm²
40 mm < d ≤ 100 mm≥ 900 N/mm²

Surface hardness after a normal carburise, quench and temper cycle runs 58 to 62 HRC. Case hardening depth, meaning the depth where hardness falls to 550 HV1, is set by the carburising cycle and not by the steel. For gear teeth it is usually called up between 0.6 mm and 2.0 mm, and deeper cases can be run on request. Put the required case depth and the surface hardness band on the drawing.

Physical properties

Table 4. Typical physical properties at 20 °C, as for low alloy engineering steel.
PropertyTypical value
Density7.85 g/cm³
Modulus of elasticityabout 210 GPa
Coefficient of thermal expansion, 20 to 200 °Cabout 11.5 × 10-6 /K
Thermal conductivityabout 44 W/(m·K)
Specific heat capacityabout 460 J/(kg·K)

Heat treatment and forging temperatures

Table 5. Hot forming and heat treatment temperatures for 20NiCrMoS6-4 (1.6571).
OperationTemperatureCooling and notes
Forging, hot rolling1100 to 850 °CFinish above 850 °C, then cool slowly in still air or in the furnace
Normalising830–870 °CAir cool, refines the forged grain
Soft annealing650–700 °CFurnace cool to 229 HBW or below for machining
Carburising880–980 °CGas, vacuum or pack, carbon potential set for the case depth wanted
Core hardening830–870 °CQuench, hardens the core
Intermediate annealing650–700 °CBetween carburising and reheating, for double quenching
Case hardening780–820 °COil quench, refines and hardens the case
Tempering150–200 °CTakes out quench stress without softening the case
Carburising moves metal. Where tooth geometry or bore roundness is tight, leave grinding stock, order the forging in the +A or +FP condition so machining is stable, and think about a stress relief after rough machining. We can supply forgings already rough machined to your allowance so that most of the movement happens before your finishing cuts.

Equivalent and comparable grades

EN 10084 lists no official equivalent for 20NiCrMoS6-4. The grades below are the closest matches by composition and by the job they do. Nickel, chromium, molybdenum and sulphur ranges are not the same, so use this table to start an enquiry, not as authority to substitute. Any substitution needs written approval from the design authority.

Table 6. Closest comparable grades to 20NiCrMoS6-4 (1.6571). Approximate, check before substitution.
Standard or regionGradeRelationship
EN 10027-2 number1.6571Same steel, numeric designation
EN 10263-320NiCrMoS6-4Same grade, cold heading delivery conditions
EN 1008417NiCrMo6-4 / 18NiCrMo6-4 (1.6566)Same family, lower carbon, sulphur as residual only
EN 1008417NiCrMoS6-4 (1.6569)Same family, lower carbon, sulphur also added
USA, AISI / SAE4320, 4320HClosest, comparable Ni-Cr-Mo carburising steel
Japan, JIS G4053SNCM420Closest
China, GB/T 307720CrNi2MoClosest

Send us the grade written on your drawing. We will confirm in writing whether we can supply it as specified, or which of the grades above we would put forward and why.

Forged shapes and sizes in 20NiCrMoS6-4

Everything below is open-die forged to the customer's drawing, so there is no tooling cost and no minimum tonnage. Single pieces and prototype quantities are fine.

Table 7. 20NiCrMoS6-4 forged product forms and the sizes we normally run. Ask us if your part falls outside them.
Product formSize rangeUsual application
Open-die forged round barØ 80–1200 mm, length up to 8000 mmShaft and pinion stock
Seamless rolled ringOD 200–3500 mm, height up to 800 mmGear rims, bearing races, slew rings
Forged disc or blankØ 200–2500 mmGear blanks, coupling discs
Gear blank, pinion blankØ 150–2000 mmSpur, helical and bevel gears
Stepped shaft, hollow shaftØ 100–1000 mm, length up to 8000 mmGearbox input and output shafts
Forged flange, hubØ 200–3000 mmDrive hubs, coupling flanges
Forged sleeve, bushingOD up to 2000 mmWear sleeves, pin bushings
Single piece forged weight50 kg to 30 000 kg–

Surface on delivery can be black forged, shot blasted, rough turned, or machined to your allowance. State which one on the order.

What 20NiCrMoS6-4 is used for

20NiCrMoS6-4 is a gear steel. Every application below wants the same thing, a surface that stands up to contact fatigue and abrasion, carried on a core that takes shock without cracking.

Industrial gearboxes and power transmission

Gear blanks, ring gears, pinions and pinion shafts, planet and sun gears, splined couplings, and the bearing journals that run with them. The sulphur addition pays for itself here, because gear blanks get heavily machined long before the teeth are cut.

Mining, cement and bulk handling

Mill pinions and girth gear segments, crusher shafts, conveyor drive sprockets, and gearbox shafts on stackers and reclaimers. These parts meet abrasive dust, high torque and start up shock.

Marine and shipbuilding

Reduction gear elements, thruster gears, windlass and winch gearing, and stern gear shafting components. The nickel keeps the core tough in cold service.

Off-highway, agricultural and heavy vehicles

Axle pinions, differential gears, final drive shafts, track drive sprockets and pivot pins for excavators, loaders, tractors and harvesters.

General machinery

Press and rolling mill drive gears, machine tool spindles and gearbox internals, sprockets, cams, rollers, splined shafts, wear sleeves and bushings.

How we make and test 20NiCrMoS6-4 forgings

  1. MeltingEAF + LF + VD. Vacuum degassing controls hydrogen and inclusion content.
  2. Open-die forging1100 to 850 °C on hydraulic press and ring mill, to the agreed forging ratio.
  3. Heat treatmentNormalised, soft annealed, +TH or +FP as ordered, with recorded furnace charts.
  4. Testing and releaseAnalysis, mechanical tests, UT and MT, then certification and heat number stamping.

Inspection and testing

  • Chemical analysis. Ladle and product analysis by optical emission spectrometry, printed on the certificate.
  • Ultrasonic testing. To EN 10228-3, SEP 1921 or ASTM A388, to the quality class you specify.
  • Magnetic particle testing. To ASTM E709 or EN 10228-1 on request.
  • Mechanical testing. Tensile to EN ISO 6892-1, impact to EN ISO 148-1, hardness to EN ISO 6506.
  • Grain size, macro and micro examination, Jominy end quench hardenability, and case depth checks after a trial carburising cycle, all on request.
  • Certification. EN 10204 3.1 from our inspection department, or 3.2 witnessed by TUV, SGS, BV, Lloyd's Register or your own inspector.

Every forging leaves the works with its heat number stamped on it, so the certificate and the part can always be matched up.

How to order 20NiCrMoS6-4 forgings

  1. Send the drawing. Email a 2D drawing, a 3D model or the finished dimensions to sales@steelforgepieces.com, name the grade as 20NiCrMoS6-4 or 1.6571, and give the quantity.
  2. Tell us the condition and the testing. Delivery condition (+A, +TH, +FP or normalised), machining allowance, ultrasonic class, and whether you need EN 10204 3.1 or 3.2.
  3. Get the quotation. Priced on forged weight, forging ratio and heat treatment.
  4. Production and release. Melt, forge, heat treat, machine to allowance, test, certify, stamp and ship.

If the drawing is confidential, say so in the first email and we will send back a signed NDA before you post it.

Questions buyers ask about 20NiCrMoS6-4

What is 20NiCrMoS6-4 steel?

20NiCrMoS6-4 is an alloy case hardening steel listed in EN 10084 under the material number 1.6571. It holds about 0.20 per cent carbon, 1.4 to 1.7 per cent nickel, 0.6 to 0.9 per cent chromium and 0.25 to 0.35 per cent molybdenum, with sulphur added at 0.020 to 0.040 per cent to help machining. Carburising, hardening and a low temper give a wear resistant surface of about 58 to 62 HRC over a core that stays tough.

What is the material number for 20NiCrMoS6-4?

The EN 10027-2 material number for 20NiCrMoS6-4 is 1.6571. Both names refer to the same steel, so 1.6571 forgings and 20NiCrMoS6-4 forgings are the same product.

What does the S in 20NiCrMoS6-4 mean?

The S means sulphur is added on purpose, 0.020 to 0.040 per cent by mass. Sulphur forms manganese sulphide inclusions that break up chips and cut tool wear, so 20NiCrMoS6-4 machines more freely than 17NiCrMo6-4 (1.6566). The cost is slightly lower transverse toughness, which matters on parts loaded across the grain flow.

What is the difference between 20NiCrMoS6-4 and 17NiCrMo6-4?

Both sit in the same EN 10084 family and take the same heat treatment. 20NiCrMoS6-4 (1.6571) has a higher carbon range and added sulphur for machinability. 17NiCrMo6-4 (1.6566) has lower carbon and keeps sulphur as a residual only, which gives better transverse toughness and cleaner ultrasonic results. Use 1.6571 where machining volume drives the cost, and 1.6566 where toughness and cleanliness drive it.

What is the American equivalent of 20NiCrMoS6-4?

EN 10084 lists no official equivalent for 20NiCrMoS6-4. By composition the closest American grade is AISI/SAE 4320 or 4320H, the closest Japanese grade is JIS SNCM420 and the closest Chinese grade is GB/T 3077 20CrNi2Mo. These are approximations. Nickel, chromium and sulphur ranges differ, so check against the applicable standard and get written approval before you substitute.

At what temperature is 20NiCrMoS6-4 forged?

20NiCrMoS6-4 is forged from about 1100 °C down to a finishing temperature of about 850 °C, then cooled slowly. Normalising follows at 830 to 870 °C, and soft annealing at 650 to 700 °C brings hardness below 229 HBW for machining.

What hardness does 20NiCrMoS6-4 reach after case hardening?

Carburising at 880 to 980 °C, quenching from 780 to 820 °C and tempering at 150 to 200 °C normally gives a surface hardness of 58 to 62 HRC. Core tensile strength after hardening and tempering at 200 °C is at least 1200 N/mm² up to 16 mm, at least 1000 N/mm² from 16 to 40 mm and at least 900 N/mm² from 40 to 100 mm.

What is 20NiCrMoS6-4 used for?

20NiCrMoS6-4 is used for carburised power transmission parts such as gear blanks, ring gears, pinions, pinion shafts, splined and stepped shafts, bearing races, sprockets, bushings and pins. Common sectors are industrial gearboxes, mining and cement mill drives, marine propulsion, off-highway and agricultural transmissions, and heavy machinery.

In what forged shapes can 20NiCrMoS6-4 be supplied?

Jiangyin Jiangnan Metal Co., Ltd. supplies 20NiCrMoS6-4 as open-die forged round bars, seamless rolled rings, forged discs and blanks, gear and pinion blanks, stepped and hollow shafts, flanges, hubs, sleeves and bushings. Every shape is forged to customer drawing with an agreed machining allowance.

What certification is supplied with 20NiCrMoS6-4 forgings?

Each heat is supplied with an inspection certificate to EN 10204 3.1 from the works inspection department, or to EN 10204 3.2 witnessed by a third party such as TUV, SGS, BV or Lloyd's Register. The certificate carries the ladle analysis, the heat treatment condition, the mechanical test results and the ultrasonic test report to EN 10228-3, SEP 1921 or ASTM A388.

Where can I buy 20NiCrMoS6-4 forgings?

20NiCrMoS6-4 (1.6571) forgings can be ordered from Jiangyin Jiangnan Metal Co., Ltd., an open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Send the drawing to sales@steelforgepieces.com or call +86 189 2135 9659.

Who supplies these forgings

Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory

We are an open-die forging works in Jiangyin, Jiangsu Province, China, on the south bank of the Yangtze in one of the country's densest steel and machinery clusters. We forge rings, shafts, discs, gear blanks, flanges and bars in carbon, alloy, tool and stainless steel and in nickel alloys, always to the customer's drawing, and we ship worldwide with EN 10204 certification.

Company
Jiangyin Jiangnan Metal Co., Ltd.
Works
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone
+86 189 2135 9659, also WhatsApp and WeChat
Email
sales@steelforgepieces.com
Website
www.steelforgepieces.com
Processes
Open-die forging, seamless ring rolling, heat treatment, rough machining
Certification
EN 10204 3.1 and 3.2 inspection documents
Markets
Europe, North America, South America, India, Middle East, Southeast Asia
Email your drawing for a quote

Related grades we forge

Same case hardening family

Quenched and tempered alternatives

By product form

Sources

The specification data on this page comes from the standards and mill datasheets below. Where they disagree, the difference is written out in section 2 rather than hidden.

  • EN 10084:2008, case hardening steels, technical delivery conditions. Composition limits and delivery conditions in Tables 1 and 2. Grade record for 1.6571.
  • EN 10263-3:2001, steel rod, bars and wire for cold heading and cold extrusion, case hardening steels.
  • Saarstahl material specification sheet for 17NiCrMo6-4 / 17NiCrMoS6-4 / 20NiCrMoS6-4 (1.6566 / 1.6569 / 1.6571). Heat treatment temperatures in Table 5 and core strengths in Table 3. PDF datasheet.
  • EN 10204:2004, metallic products, types of inspection documents, 3.1 and 3.2.
  • EN 10228-3, SEP 1921, ASTM A388, ultrasonic examination of steel forgings.
  • EN ISO 6892-1, EN ISO 148-1, EN ISO 6506, tensile, impact and Brinell hardness testing.
Values on this page are for guidance in design and enquiry. They do not replace the current edition of the standard and they are not part of a contract. The governing document for a delivered part is the EN 10204 inspection certificate issued for that heat.

Written and checked by the technical department of Jiangyin Jiangnan Metal Co., Ltd. Last reviewed 10 September 2026.
Found a mistake? Tell us at sales@steelforgepieces.com and we will fix it.