Jiangyin Jiangnan Metal Co., Ltd., Open-Die Forging Factory, Jiangyin, Jiangsu, China | Tel 0086-189-2135-9659 | Email sales@steelforgepieces.com
Jiangyin Jiangnan Metal Co., Ltd. Open-Die Forgings and Seamless Rolled Rings
Nitrogen-strengthened austenitic stainless steel, ASTM A182 F316N

UNS S31651 (AISI 316N) Open-Die Forgings: Composition, Properties and Product Range

Published 12 March 2019. Last reviewed 21 September 2026. Maintained by the technical department of Jiangyin Jiangnan Metal Co., Ltd., an open-die forging factory in Jiangyin, Jiangsu, China.

UNS S31651 is the Unified Numbering System number for AISI Type 316N, a nitrogen-strengthened, molybdenum-bearing austenitic stainless steel. The composition limits are 16.0 to 18.0 % chromium, 10.0 to 14.0 % nickel, 2.00 to 3.00 % molybdenum and 0.10 to 0.16 % nitrogen, with carbon held to 0.08 % maximum and iron as the balance.

Nitrogen strengthens the alloy by interstitial solid solution. It lifts the specified minimum yield strength from 205 MPa (30 ksi) for Type 316 to 240 MPa (35 ksi), and the minimum tensile strength from 515 MPa to 550 MPa (80 ksi). Carbon is not raised to achieve this, so weldability and chloride behaviour stay close to standard 316. The higher minimums give a higher ASME allowable stress, which lets a designer use a thinner wall on a flange hub, valve body or vessel nozzle.

Jiangyin Jiangnan Metal Co., Ltd. is an open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. We forge UNS S31651 into round, square and flat bars, hollow bars and sleeves, seamless rolled rings, discs, blocks, shafts, spindles and flanges. Material is supplied solution annealed with EN 10204 3.1 or 3.2 certification.

  • UNS numberS31651
  • Common nameAISI 316N
  • Forging specASTM A182 F316N
  • Tensile, min550 MPa (80 ksi)
  • Yield 0.2 %, min240 MPa (35 ksi)
  • Elongation, min30 % in 50 mm
  • Density7.98 g/cm³
  • PREN24 to 31 typ. 27
  • Solution anneal1040 to 1100 °C
  • ConditionSolution annealed

1. What UNS S31651 is and why nitrogen is added

UNS S31651 sits in the 18-8 austenitic family, on the molybdenum-bearing 316 branch. Molybdenum at 2 to 3 % holds the passive film against chloride attack. Chromium at 16 to 18 % forms that film. Nickel at 10 to 14 % keeps the structure fully austenitic and tough down to cryogenic temperature. What separates S31651 from plain 316 is a controlled nitrogen range of 0.10 to 0.16 %.

Nitrogen dissolves in the austenite lattice as an interstitial. Per weight percent it is one of the strongest solid solution strengtheners available in stainless steel, roughly ten times more effective than nickel or molybdenum. It does not form chromium carbides at grain boundaries the way carbon does, so the added strength costs nothing in intergranular corrosion resistance. Nitrogen also adds to the pitting resistance equivalent, and it makes the austenite more stable against strain-induced martensite during cold work.

Design codes are where this shows up in practice. ASME allowable stresses come from the specified minimum yield and tensile values, so moving from 205 MPa to 240 MPa minimum yield lets a designer take wall thickness out of a flange hub, valve body or nozzle. On a large forging, removing 10 % of the wall can take several hundred kilograms out of the part, which shows up in material cost, machining hours and freight.

Naming. UNS S31651, AISI Type 316N, ASTM A182 Grade F316N, ASME SA-182 F316N, JIS SUS316N and GB/T 06Cr17Ni12Mo2N all designate the same alloy. Which specification you order to depends on the product form and the code the component is built to.

2. Chemical composition limits of UNS S31651

The composition below is the specification window for UNS S31651 given in ASTM A182/A182M Grade F316N and ASTM A240 Type 316N. Values are weight percent on the heat analysis. Product analysis tolerances apply per the governing standard, and iron is the balance.

Table 1. Chemical composition limits, UNS S31651 (AISI 316N), wt %
ElementSymbolMinimumMaximumRole in the alloy
CarbonC–0.080Strength. Held low to limit carbide sensitisation
ManganeseMn–2.00Deoxidiser. Raises nitrogen solubility
PhosphorusP–0.045Residual. Restricted for hot ductility
SulfurS–0.030Residual. Restricted for forgeability
SiliconSi–0.75Deoxidiser. Aids oxidation resistance
ChromiumCr16.0018.00Forms the passive chromium oxide film
NickelNi10.0014.00Stabilises austenite. Low-temperature toughness
MolybdenumMo2.003.00Pitting and crevice corrosion resistance
NitrogenN0.100.16Solid solution strengthening. Raises PREN
IronFeBalance, approx. 61.9 to 71.9Matrix

Melt practice. Billet for UNS S31651 forgings is procured to AOD, or AOD plus ESR where the specification calls for it. We verify nitrogen recovery by product analysis on the finished forging rather than relying on the ladle certificate alone, because nitrogen can be lost during long soaking at forging temperature. If your specification imposes a narrower nitrogen band, for example 0.12 to 0.16 % for allowable stress reasons, agree it at order entry and it will appear on the mill test certificate.

3. Mechanical properties of UNS S31651 forgings

Table 2 gives the specified minimum room-temperature requirements for forged UNS S31651 in the solution-annealed condition, per ASTM A182/A182M Grade F316N. Production heats normally exceed these minimums. The typical column reflects values reached on solution-annealed forged sections up to about 200 mm ruling section.

Table 2. Room-temperature mechanical properties, UNS S31651 forgings, solution annealed
PropertyASTM A182 F316N minimumTypical as produced
Tensile strength, Rm550 MPa (80 ksi)590 to 680 MPa
Yield strength, Rp0.2240 MPa (35 ksi)270 to 340 MPa
Elongation in 50 mm, A30 %40 to 55 %
Reduction of area, Z50 %60 to 75 %
Hardness217 HBW max (96 HRB max)150 to 190 HBW
Charpy V impact at −196 °CNot required by A18280 J and above, on request
Modulus of elasticity, E–193 to 200 GPa
Poisson's ratio–0.27 to 0.30

Strength at temperature

Like all austenitic stainless steels, UNS S31651 gives up a large part of its room-temperature yield strength as temperature rises, then holds a broad plateau. The nitrogen contribution carries across that plateau, which is why 316N carries higher ASME Section II Part D allowable stresses than 316 over most of the useful range. Table 3 gives indicative minimum yield values for screening work only.

Table 3. Indicative elevated-temperature minimum yield strength, UNS S31651, for screening only
Temperature100 °C200 °C300 °C400 °C500 °C
Rp0.2, MPa, approx.205175160150145

Design note. Table 3 is for preliminary screening. Allowable stress values for pressure-retaining components must be taken from ASME BPVC Section II Part D, EN 13445-2 or the governing design code for the actual product form and thickness. We supply material to specification and do not carry out pressure-vessel design.

4. Physical and thermal properties

Table 4. Physical properties of UNS S31651 (AISI 316N), solution annealed
PropertyMetricImperial
Density7.98 g/cm³0.288 lb/in³ (498 lb/ft³)
Melting range1370 to 1400 °C2500 to 2550 °F
Modulus of elasticity at 20 °C193 to 200 GPa28 to 29 × 106 psi
Thermal conductivity at 100 °C15 W/m·K104 BTU·in/h·ft²·°F
Specific heat capacity at 20 °C500 J/kg·K0.12 BTU/lb·°F
Thermal expansion, 0 to 100 °C16.0 µm/m·K8.9 µin/in·°F
Thermal expansion, 0 to 500 °C17.5 µm/m·K9.7 µin/in·°F
Electrical resistivity at 20 °C0.74 µΩ·mapprox. 2.4 % IACS
Relative magnetic permeabilitybelow 1.02, annealedNon-magnetic

Two of these numbers cause most fabrication trouble. Thermal conductivity of 15 W/m·K is about a third that of carbon steel, so heat does not leave the cut zone during machining. Rigid setups, positive rake, sharp tooling and generous coolant all follow from that. Thermal expansion of 16.0 µm/m·K is roughly 40 % higher than carbon steel, so weld shrinkage and distortion on large assemblies are greater, and machining allowances on long shafts have to account for it.

5. Corrosion resistance and PREN of UNS S31651

The pitting resistance equivalent number is calculated with the nitrogen-weighted formula:

PREN = %Cr + 3.3 × %Mo + 16 × %N

At minimum composition, 16.0 Cr, 2.00 Mo, 0.10 N: PREN is about 24.2.
At a mid-range heat, 17.0 Cr, 2.50 Mo, 0.13 N: PREN is about 27.3.
At maximum composition, 18.0 Cr, 3.00 Mo, 0.16 N: PREN is about 30.5.

For comparison, standard Type 316 with no nitrogen addition falls around 24 to 25, Type 304 around 18 to 20, and super-austenitic A182 F44 (UNS S31254, 6Mo) around 43. UNS S31651 therefore sits between plain 316 and the high-alloy grades. It gives better chloride pitting resistance than 316 at close to the same alloy cost, but it does not reach what 6Mo or super duplex grades deliver.

Where UNS S31651 works well

  • Sulfuric, phosphoric and organic acids at moderate concentration and temperature, where molybdenum is the deciding element.
  • Neutral and mildly acidic chloride waters, including seawater at ambient temperature for intermittent service.
  • Mildly sour hydrocarbon streams, subject to NACE MR0175 and ISO 15156 qualification of the specific component.
  • Cryogenic duty to −196 °C, where austenite stability keeps impact toughness high and the nitrogen strengthening is retained.

Where it should not be used

  • Hot chloride stress corrosion cracking. Above roughly 60 °C in chloride service under tensile stress, all 300-series austenitics including 316N are at risk. Duplex grades such as A182 F51 (UNS S31803) or A182 F53 (UNS S32750) are the correct choice there.
  • Warm seawater or concentrated brine. Specify 904L or a 6Mo grade instead.
  • Heavy welded sections that will sit between 425 and 815 °C and cannot be re-solution annealed. Specify 316L or 316LN (UNS S31653), which cap carbon at 0.030 %.

6. International equivalent grades for UNS S31651

Table 5. Cross-reference of UNS S31651 (AISI 316N) across standards
Standard or regionDesignationMatchNote
UNS, USAS31651ExactReference designation
AISI / ASTM, USAType 316NExactGrade name
ASTM A182 / ASME SA-182F316NExactForged flanges, fittings, valves
ASTM A240316NExactPlate, sheet, strip
ASTM A276 / A479316NExactBars and shapes
JIS, JapanSUS 316NExactJIS G 4303, G 4304
GB/T, China06Cr17Ni12Mo2N
formerly 0Cr17Ni12Mo2N
ExactGB/T 1220, GB/T 20878
EN, Europe1.4406 / X2CrNiMoN17-11-2
1.4429 / X2CrNiMoN17-13-3
Nearest onlyBoth are 316LN: nitrogen alloyed, carbon 0.030 % max. No exact EN counterpart to 316N exists
AFNOR, FranceZ3 CND 17-12 AzNearestLow-carbon nitrogen grade
BS, UK, withdrawn316 S 62NearestSuperseded by EN designations
ISOX2CrNiMoN17-12-2NearestISO 15510

Substitution warning. There is no exact European equivalent to UNS S31651. Both 1.4406 and 1.4429 restrict carbon to 0.030 % maximum, which makes them 316LN rather than 316N. Substituting them is usually conservative, since lower carbon improves sensitisation resistance while nitrogen keeps the strength, but it remains a deviation that the design authority has to approve in writing before material is released. Tell us at enquiry stage and the deviation will be stated on the certificate instead of left implied.

7. UNS S31651 against 316, 316L and 316LN

The four grades in Table 6 differ only in carbon and nitrogen, but that difference decides which one a code-stamped component can use.

Table 6. Comparison of the four members of the 316 family
GradeUNSC max, %N, % Yield min, MPaTensile min, MPaBest suited to
316S316000.08–205515General corrosion service, machined parts
316LS316030.030–170 to 205485 to 515Heavily welded assemblies, no post-weld anneal
316NS316510.080.10 to 0.16240550Pressure parts needing higher allowable stress
316LNS316530.0300.10 to 0.16240550Welded pressure parts, nuclear service

Selection follows from the fabrication route. A component machined from a forging and welded lightly or not at all gets the strength most cheaply from 316N. A component welded in heavy section that cannot be re-solution annealed afterwards should move to 316LN and accept the premium for lower carbon. Where neither strength nor heavy welding is the driver, plain 316 or 316L is enough. We forge all four. If you are not sure which one your drawing needs, send the drawing and the service conditions and we will advise before you order.

8. UNS S31651 forged product forms and size range

Jiangyin Jiangnan Metal produces UNS S31651 by open-die forging and seamless ring rolling. Open-die forging is used instead of casting or plate fabrication because the reduction ratio breaks down the as-cast dendritic structure, closes porosity and aligns grain flow with the loaded direction. That is what gives a forged flange hub or valve body its through-thickness properties.

Round, square, flat and hex bars

Forged round bars 80 to 1,200 mm diameter. Square, rectangular, flat and hexagonal sections. Lengths to 8,000 mm. Black forged, rough turned, or peeled and polished.

Hollow bars, sleeves and bushings

Bored and trepanned hollows, sleeves, bushings, cylinders, casings, shells, hubs and housings. Outside diameter 150 to 2,500 mm, inside diameter from 100 mm.

Seamless rolled rings

Radial and axial rolled rings, outside diameter 200 to 4,000 mm, wall from 40 mm, height to 1,500 mm. Rectangular and contour-rolled profiles.

Discs, blocks and plates

Forged discs to 3,000 mm diameter. Blocks and slabs to 800 mm thickness, upset and cross forged for balanced grain flow.

Shafts and spindles

Straight and stepped shafts, spindles and rotors to 8,000 mm length, with integral collars and flanged ends.

Flanges and near-net shapes

Forged flange blanks to ASME B16.5 and B16.47, weld neck, blind, slip-on and special bores. Custom near-net preforms to drawing.

Minimum order quantity is one piece, including a single prototype forging. Material can be supplied black forged, rough machined to your allowance, or finish machined to drawing.

9. Forging and heat-treatment practice for UNS S31651

Table 7. Processing parameters for UNS S31651 open-die forgings
OperationParameterReason
Pre-heat and soakSlow to 850 °C, then to forging heatLow thermal conductivity. Avoids thermal cracking in heavy sections
Forging start temperature1150 to 1230 °CUpper limit avoids incipient melting and delta ferrite
Finish forging temperatureNot below 925 °CPrevents carbide precipitation and hot tearing on the last blows
Minimum reduction ratio3:1 typical, 4:1 for critical partsBreaks down as-cast structure and closes centreline porosity
Cooling after forgingAir coolNo transformation hardening in austenitic steel
Solution annealing1040 to 1100 °C, soak, rapid water quenchDissolves carbides and restores full corrosion resistance
Quench delayAs short as practicable through 815 to 425 °CThe sensitisation band. Slow cooling here precipitates Cr23C6
Stress reliefNot normally appliedAny treatment in the sensitisation band would undo the anneal
DescalingPickle and passivateRemoves forge scale and free iron from the surface

Machining guidance

UNS S31651 work-hardens faster than 316 because nitrogen raises the work-hardening rate. Use rigid setups, positive rake carbide tooling, moderate surface speed and a heavy uninterrupted feed. Feeding too lightly lets the tool ride on and burnish the work-hardened layer, which destroys tool life. Use flood coolant and do not allow the tool to dwell in the cut.

10. Applications of UNS S31651 forgings by industry

Oil, gas and petrochemical

Weld neck and blind flanges, valve bodies and bonnets, wellhead components, separator nozzles and pipeline fittings to ASTM A182 F316N.

Chemical process plant

Reactor nozzles, agitator shafts, pump casings and impellers, heat exchanger tubesheets and channel covers in sulfuric, phosphoric and organic acid duty.

Marine and desalination

Pump shafts and sleeves, propeller shaft components, seawater valve internals and high-pressure pump parts for reverse osmosis trains.

Power generation

Pressure boundary fittings, pump and valve internals, and support hardware where a nitrogen-strengthened 316 variant is the code-specified choice.

Pulp, paper and food processing

Digester and bleach plant hardware, roll journals, and hygienic pressure vessel components needing a smooth passivated surface.

Cryogenic and LNG

Valve bodies, flanges and pump parts for service to −196 °C, where austenite stability keeps impact toughness high.

11. Testing, NDT and certification

Every UNS S31651 forging is released against a documented test package. The standard scope is listed below. Additional or witnessed testing is added at order entry.

Table 8. Standard test and inspection scope for UNS S31651 forgings
TestMethod or standardScope
Chemical analysisOptical emission spectrometry, nitrogen by inert gas fusionHeat and product analysis
Tensile testASTM A370, ISO 6892-1Per heat and heat-treatment lot
HardnessASTM E10 BrinellEach piece
Impact testASTM A370 Charpy V, ambient or cryogenicOn request
Intergranular corrosionASTM A262 Practice E (Strauss)On request. Practice A, B and C available
Ultrasonic examinationASTM A388, EN 10228-3Standard on rings, discs and shafts
Liquid penetrant examinationASTM E165, EN 10228-2Machined surfaces, on request
Positive material identificationPortable XRFOn request, marked per piece
Grain size and microstructureASTM E112On request
Ferrite contentFeritscope or metallographicOn request
Dimensional reportPer customer drawingEach piece
CertificationEN 10204 3.1 standard. 3.2 with TUV, SGS, BV, Lloyd's Register or customer inspectorEvery order

Heat traceability runs from the billet certificate through forging travellers, heat-treatment charts and final release, so any piece can be traced back to its heat number and anneal cycle.

12. How to specify a UNS S31651 enquiry

Quotations are fastest and most accurate when the enquiry states the following. A drawing covers most of it, so if you have one, send the drawing and the service conditions and nothing else is needed.

  1. Grade and specification. UNS S31651, and the governing standard: ASTM A182 F316N, ASTM A479 316N, or your own material specification number.
  2. Product form and dimensions. Bar, ring, disc, shaft, sleeve or flange, with finished dimensions and the machining allowance to be left on.
  3. Quantity and delivery date. Piece count and required arrival date, not ex-works date.
  4. Delivery condition. Black forged, rough turned, or finish machined to drawing.
  5. Testing requirements. Tensile, impact temperature, ASTM A262 practice, UT acceptance class, PMI, witnessed or not.
  6. Certification. EN 10204 3.1 or 3.2, and which third party if 3.2.
  7. Marking, packing and destination port. Heat number marking method, and whether seaworthy wooden cases are required.

13. Frequently asked questions about UNS S31651

What is UNS S31651?

UNS S31651 is the Unified Numbering System number for AISI Type 316N, a nitrogen-strengthened molybdenum-bearing austenitic stainless steel. The composition limits are 16.0 to 18.0 % chromium, 10.0 to 14.0 % nickel, 2.00 to 3.00 % molybdenum, 0.10 to 0.16 % nitrogen and 0.08 % carbon maximum, with iron as the balance. In forged form it is ordered as ASTM A182 or ASME SA-182 Grade F316N.

Is UNS S31651 the same as 316N?

Yes. UNS S31651, AISI 316N, Type 316N and ASTM A182 F316N all name the same alloy. UNS S31651 is the numeric designation, 316N is the AISI and ASTM grade name, and F316N is the forging grade symbol used in ASTM A182.

What is the difference between 316N and 316L?

316N (UNS S31651) contains 0.10 to 0.16 % nitrogen and allows carbon up to 0.08 %, giving a specified minimum yield strength of 240 MPa. 316L (UNS S31603) has no deliberate nitrogen addition and holds carbon to 0.030 %, giving a minimum yield of 205 MPa. Use 316N when higher code allowable stress is the driver. Use 316L when resistance to weld sensitisation is the driver. 316LN (UNS S31653) gives both.

What ASTM standard covers UNS S31651 forgings?

Forged UNS S31651 is supplied to ASTM A182/A182M Grade F316N, or the ASME Boiler and Pressure Vessel Code equivalent SA-182 F316N, covering forged flanges, fittings, valves and parts for high-temperature service. Plate and sheet fall under ASTM A240 Type 316N. Bars and shapes fall under ASTM A276 and A479.

What is the PREN of UNS S31651?

Using PREN = %Cr + 3.3 × %Mo + 16 × %N, UNS S31651 gives about 24 at minimum composition and about 31 at maximum, with a typical heat around 27. That is several points above plain Type 316, entirely because of the nitrogen term.

Is UNS S31651 magnetic?

No. In the solution-annealed condition it is fully austenitic and non-magnetic, with relative permeability normally below 1.02. Nitrogen and nickel stabilise the austenite, so it resists strain-induced martensite better than Type 304. Heavy cold work can produce a slight local magnetic response.

Can UNS S31651 be welded?

Yes. It welds by GTAW, SMAW, GMAW and SAW without preheat. ER316L and E316L-16 consumables are common. Where the weld metal has to match the nitrogen-enhanced strength of the base material, a nitrogen-alloyed filler such as ER316LMn is specified. Because carbon can reach 0.08 %, long exposure between 425 and 815 °C can sensitise heavy sections, so 316LN is preferred for thick welded assemblies that cannot be re-solution annealed.

What is the EN or DIN equivalent of UNS S31651?

There is no exact EN equivalent. The closest grades are 1.4406 (X2CrNiMoN17-11-2) and 1.4429 (X2CrNiMoN17-13-3), both nitrogen alloyed but with carbon restricted to 0.030 % maximum, which makes them 316LN rather than 316N. Confirm with your design authority before substituting.

What is the maximum service temperature of UNS S31651?

Oxidation resistance in air is adequate to roughly 870 °C in continuous service and about 925 °C intermittently. For pressure-retaining components, ASME Section II Part D lists allowable stresses well into the 800 °C range, but with carbon permitted to 0.08 % long exposure between 425 and 815 °C risks carbide sensitisation. Where long-term service falls in that band, specify 316LN.

What forged shapes are available in UNS S31651?

We supply UNS S31651 as forged round, square, rectangular, flat and hexagonal bars, hollow bars, sleeves, bushings, cylinders, casings and shells, seamless rolled rings, forged rings, discs, blocks and plates, and shafts, spindles and flanges. Minimum order quantity is one piece.

What certification is supplied?

Every order ships with an EN 10204 3.1 mill test certificate as standard, covering heat chemistry, mechanical results, the solution-annealing record, the dimensional report and NDT results. EN 10204 3.2 with third-party inspection by TUV, SGS, BV, Lloyd's Register or your own inspector is available on request.

What is the lead time for UNS S31651 forgings?

Lead time depends on size, whether billet is in stock, heat-treatment lot scheduling and the testing scope. Send dimensions, quantity and test requirements to sales@steelforgepieces.com and we will confirm a date with the quotation.

Request a UNS S31651 quotation

Send a drawing, or the grade, shape, dimensions and quantity. Enquiries received during Chinese business hours are normally answered the same working day.

  • Jiangyin Jiangnan Metal Co., Ltd., Open-Die Forging Factory
  • No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
  • Telephone, WhatsApp and WeChat: 0086-189-2135-9659
  • Email: sales@steelforgepieces.com

Email the forging team   Full contact details