UNS R20033 Forgings: Alloy 33 / 1.4591 Bars, Rolled Rings, Flanges and Discs
Published by Jiangyin Jiangnan Metal Co., Ltd., Jiangyin, Jiangsu, China · Last reviewed · Data from ASTM B462, B649, B625 and B622, VdTÜV Sheet 516 and the published alloy development work listed under references.
UNS R20033 is a nitrogen-alloyed high-chromium austenitic alloy with nominally 33 % chromium, 31 % nickel, 32 % iron, 1.6 % molybdenum, 0.6 % copper and 0.4 % nitrogen. The same material carries the designations W.Nr. 1.4591, X1CrNiMoCuN33-32-1, Alloy 33 and Nicrofer 3033. It came to market in 1995 for duty that defeats ordinary austenitic and super-austenitic grades: hot concentrated sulphuric acid, nitric acid and HNO3/HF mixtures. Its resistance rests on chromium rather than molybdenum. The nitrogen gives a fine grain size after solution annealing, which raises proof strength while keeping impact toughness high.
Jiangyin Jiangnan Metal Co., Ltd. melts and forges UNS R20033 in one works at Jiangyin, Jiangsu, China. Products are forged round bar, square, flat and hex bar, seamless rolled rings, flanges, discs, blocks, hollow bars and sleeves, made to ASTM B462, ASTM B649 or customer drawing, solution annealed and supplied with EN 10204 3.1 or 3.2 certificates. Contact sales@steelforgepieces.com or 0086-189-2135-9659.
- UNS
- R20033
- Werkstoff No.
- 1.4591
- EN name
- X1CrNiMoCuN33-32-1
- Trade names
- Alloy 33, Nicrofer 3033
- Chromium
- 31.0–35.0 %
- Nitrogen
- 0.35–0.60 %
- Rp0.2 (VdTÜV 516)
- ≥ 380 MPa
- Density
- 7.9 g/cm³
- Solution anneal
- 1100–1150 °C
- Forgings standard
- ASTM B462
1. Designations and standards
Enquiries for this alloy arrive under at least five different names, which is a common source of ordering mistakes. All of the entries in Table 1 refer to one material.
| System | Designation |
|---|---|
| UNS | R20033 |
| Werkstoff number | 1.4591 |
| EN steel name | X1CrNiMoCuN33-32-1 |
| Trade names | Alloy 33, Nicrofer 3033 |
| Welding consumable | AWS A5.9 ER33-31, ISO 14343-A S Z 33 32 1 Cu N L |
| GB/T (China) | No direct national equivalent. Supplied to the ASTM or EN designation. |
Some distributors quote UNS N08033 for this alloy. ASTM specifications use R20033. Our page for the European designation is 1.4591 forgings, which carries the same data under the EN name.
| Product form | ASTM | ASME | European |
|---|---|---|---|
| Forged flanges, fittings, valves and parts | B462 | SB-462 | VdTÜV 516 |
| Bar, rod and wire | B649 | SB-649 | VdTÜV 516 |
| Plate, sheet and strip | B625 | SB-625 | EN 10029, VdTÜV 516 |
| Seamless pipe and tube | B622 | SB-622 | – |
| Welded pipe | B619 | SB-619 | – |
| Pressure-vessel service range | −196 °C to 450 °C (−320 to 840 °F) | ||
For forged parts the governing document is normally ASTM B462, whose title names UNS R20033 directly alongside the nickel alloys. We forge against B462 with the chemistry, mechanical testing and heat-treatment records it calls for.
2. Chemical composition of UNS R20033
Iron is the balance, around 32 %.
| Element | Symbol | Min. | Max. | Nominal |
|---|---|---|---|---|
| Chromium | Cr | 31.0 | 35.0 | 33 |
| Nickel | Ni | 30.0 | 33.0 | 31 |
| Iron | Fe | Balance | 32 | |
| Molybdenum | Mo | 0.50 | 2.00 | 1.6 |
| Nitrogen | N | 0.35 | 0.60 | 0.4 |
| Copper | Cu | 0.30 | 1.20 | 0.6 |
| Manganese | Mn | – | 2.00 | – |
| Silicon | Si | – | 0.50 | – |
| Carbon | C | – | 0.015 | 0.010 |
| Phosphorus | P | – | 0.020 | – |
| Sulphur | S | – | 0.010 | – |
Three parts of that analysis decide how the alloy behaves in service and in the shop.
- Chromium at about 33 %. The passive film stays stable in strongly oxidising acid that attacks molybdenum-rich alloys. This inverts the usual super-austenitic logic, where molybdenum carries the corrosion load.
- Nitrogen at about 0.4 %. Held in solution by 31 % nickel, it keeps the structure fully austenitic, refines the grain after solution annealing and lifts minimum proof strength to 380 MPa under VdTÜV 516.
- Copper and molybdenum. The 0.6 % copper helps passivation in sulphuric acid. The 1.6 % molybdenum improves behaviour in phosphoric acid and adds to pitting resistance.
Carbon stays below 0.015 % to hold back chromium-carbide precipitation at grain boundaries. Ageing for up to eight hours anywhere between 600 °C and 1000 °C does not sensitise the alloy when checked by boiling azeotropic nitric acid, which leaves working margin during welding and hot work.
3. Mechanical properties
Two sets of numbers circulate for this alloy and they are not interchangeable. An ASTM product specification sets a floor that the material is formally accepted against. VdTÜV 516 and the alloy producer data sheet give higher guaranteed values for solution-annealed material. Both appear below, each labelled with its source. Design to the document named on your drawing, and name that document on the purchase order.
| Source | Product form | Rm, min | Rp0.2, min | A, min |
|---|---|---|---|---|
| ASTM B625 | Plate, sheet, strip | 600 MPa (87 ksi) | 295 MPa (43,000 psi) | 40 % |
| ASTM B622 | Seamless pipe and tube | 750 MPa | 380 MPa | – |
| VdTÜV 516 / producer data sheet | Sheet and plate ≤ 50 mm; bar ≤ 150 mm, solution annealed | 720–920 MPa | 380 MPa (55.1 ksi) | 40 % |
Rp1.0 under VdTÜV 516 is at least 420 MPa (60.9 ksi). A dash marks a value we hold no verified figure for, not an absence of requirement. Minimums for forgings under the current edition of ASTM B462 are confirmed at order review, and we will quote the governing table for your product form and section on request.
| Temperature | Rp0.2 | Rp1.0 |
|---|---|---|
| 20 °C (68 °F) | 380 MPa | 420 MPa |
| 100 °C (212 °F) | 320 MPa | 350 MPa |
| 200 °C (392 °F) | 270 MPa | 300 MPa |
| 300 °C (572 °F) | 240 MPa | 270 MPa |
| 400 °C (752 °F) | 220 MPa | 250 MPa |
| 500 °C (932 °F) | 210 MPa | 240 MPa |
| Property | Condition | Value |
|---|---|---|
| Brinell hardness | Sheet ≤ 50 mm, strip ≤ 3 mm, bar ≤ 150 mm | ≤ 240 HBW |
| ISO-V impact energy, 20 °C | Sheet | ≥ 150 J (111 ft·lbf) |
| ISO-V impact energy, 20 °C | Bar and forgings | ≥ 120 J |
Weld metal laid with matching filler reaches impact toughness close to wrought plate, with no measured loss in the heat-affected zone. That result is the reason the alloy is accepted for welded pressure equipment.
4. Physical properties
| Property | Metric | Imperial |
|---|---|---|
| Density | 7.9 g/cm³ | 0.285 lb/in³ |
| Melting range | 1330–1370 °C | 2430–2498 °F |
| Modulus of elasticity | 195 GPa | 28.3 × 10³ ksi |
| Thermal conductivity | 13.4 W/(m·K) | 7.74 Btu·in/(ft²·h·°F) |
| Specific heat capacity | 446 J/(kg·K) | 0.107 Btu/(lb·°F) |
| Electrical resistivity | 104 µΩ·cm | 104 µΩ·cm |
| Relative magnetic permeability | 1.01 | 1.01 |
| Crystal structure | Face-centred cubic | Fully austenitic |
| T | Specific heat J/(kg·K) | Thermal cond. W/(m·K) | Resistivity µΩ·cm | E-modulus GPa | Mean CTE 10⁻⁶/K |
|---|---|---|---|---|---|
| 20 °C | 446 | 13.4 | 104 | 195 | – |
| 100 °C | 466 | 14.6 | 107 | 185 | 14.5 |
| 200 °C | 486 | 16.0 | 109 | 176 | 15.3 |
| 300 °C | 503 | 17.5 | 112 | 170 | 15.3 |
| 400 °C | 520 | 19.0 | 114 | 163 | 15.7 |
| 500 °C | 538 | 20.4 | 116 | 159 | 16.1 |
Thermal conductivity of 13.4 W/(m·K) is low and expansion is higher than carbon steel. Both facts matter when setting weld sequence and fixturing on large rings and tubesheets.
5. Corrosion resistance and PREN
The alloy was built for oxidising duty. Its chromium content holds a passive film in media that dissolve molybdenum-rich nickel alloys, while nitrogen and the modest molybdenum give chloride pitting resistance on a par with 6 % Mo super-austenitic steel. It also resists alkaline media and chloride-induced stress-corrosion cracking.
Pitting resistance equivalent number
From the nominal analysis of 33 Cr, 1.6 Mo and 0.4 N:
- PREN = %Cr + 3.3 × %Mo + 16 × %N = 33 + 5.28 + 6.4 = 44.7
- PREN = %Cr + 3.3 × %Mo + 30 × %N = 33 + 5.28 + 12.0 = 50.3
Both formulas see use. The 16×N version is the conservative one and the figure usually quoted in specifications. Seawater duty normally calls for PREN above 40, which the alloy clears on either calculation. Recalculate from the mill certificate for each heat, since chemistry moves inside the specified limits.
Measured corrosion rates
| Medium and duration | Temperature | Rate |
|---|---|---|
| H2SO4 98 %, 7 days | 100 °C | 0.04 mm/a |
| H2SO4 98 %, 7 days | 125 °C | 0.07 mm/a |
| H2SO4 98 %, 7 days | 150 °C | 0.08 mm/a |
| H2SO4 98 %, 7 days | 175 °C | 0.16 mm/a |
| H2SO4 98 %, 7 days | 200 °C | 0.04 mm/a |
| H2SO4 99.1 %, 134 days, flow > 1.2 m/s | 150 °C | < 0.01 mm/a |
| H2SO4 96–98.5 %, 14 days, flow > 1 m/s | 135–140 °C | < 0.01 mm/a |
| H2SO4 96 %, 65 days, SO2-saturated | 80 °C | 0.06 mm/a |
| H2SO4 96 % with nitrosylsulphuric acid, 7 days | 240 °C | 0.33 mm/a |
| Medium | Temperature | Rate |
|---|---|---|
| H3PO4 85 % | 100 °C | 0.08 mm/a |
| H3PO4 85 % | 154 °C | 1.07 mm/a |
| NaOH 25 % | 75 °C and boiling | < 0.01 mm/a |
| NaOH 50 % | 75 °C, 100 °C, boiling | < 0.01 mm/a |
| HNO3 12 % | 90 °C | < 0.01 mm/a |
| HNO3 12 % + HF 0.9 % | – | 0.24 mm/a |
| HNO3 32 % + HF 0.4 % | – | 0.27 mm/a |
| HNO3 45 % + HF 0.4 % | – | 0.67 mm/a |
| HNO3 68 % + HF 0.4 % | – | 3.08 mm/a |
Rates describe the stated test conditions. They are not a guarantee for any particular plant stream, and phosphoric acid above 150 °C shows how fast the picture can change with temperature.
Surface condition decides field performance. The alloy reaches its published resistance only when the surface is clean and metallically bright. Forging scale, grinding burn, embedded iron and weld heat tint all cut resistance. Every R20033 forging leaving our works is solution annealed and descaled, and pickled where the order calls for it.
6. Where the alloy is used
| Industry or duty | Application | Forgings normally needed |
|---|---|---|
| Sulphuric acid | Heat recovery and acid distribution, pipework and exchangers for acid carrying chlorides | Flanges, tubesheets, valve bodies, blocks |
| Nitric and HF service | Storage and transport vessels for HNO3/HF mixtures, pickling lines | Rolled rings, flanges, nozzles, hollow bars |
| Seawater and desalination | Seawater pipework, condensers, coolers | Rolled rings, flanges, pump shafts, sleeves |
| Chlor-alkali | NaOH and KOH to 70 wt.% and 170 °C maximum | Flanges, discs, valve internals |
| Fertiliser and urea | Urea solutions from 5 to 90 wt.% | High-pressure flanges, forged fittings, blocks |
| Pulp and paper | Bleach plant for chemical pulp, recovery equipment | Rings, shafts, sleeves |
| PTA plants | Vessels and piping in purified terephthalic acid service | Flanges, forged fittings, discs |
| Heat transfer | Plate and tubular exchangers on brackish water or seawater, salt and alkali evaporators | Tubesheets, flanges, discs |
7. Forging and heat treatment
R20033 takes open-die forging and ring rolling, but the window is tighter than for 304 or 316. Below is the route we follow.
Cleanliness before the furnace
The billet must be free of sulphur, phosphorus, lead and other low-melting metals before it is charged. These embrittle the alloy at forging heat, and they arrive through marking paint, temperature crayons, grease, oil and fuel. We keep fuel sulphur as low as the burner allows and prefer electric furnaces, which hold temperature closely and add no combustion products.
Furnace atmosphere
Hold the atmosphere neutral to slightly oxidising. Do not let it swing between oxidising and reducing, and keep flame off the workpiece.
Hot work
Charge into a furnace already at temperature, 1200 °C maximum, and forge from 1200 °C down to 1000 °C (2192 to 1832 °F). Cool quickly once the shape is finished. Finishing below 1000 °C invites cracking, because the alloy is strong hot and work-hardens quickly.
Solution annealing
Heat treatment after hot work is not optional where corrosion matters. Solution anneal between 1100 and 1150 °C (2012 to 2102 °F), around 1120 °C by preference, charging into a hot furnace, then water quench. Soak time runs from the moment the section reaches temperature.
| Thickness | Soak time t | Example |
|---|---|---|
| d < 10 mm | t = d × 3 min/mm | 8 mm → 24 min |
| d = 10–20 mm | t = 30 min + (d − 10) × 2 min/mm | 16 mm → 42 min |
| d > 20 mm | t = 50 min + (d − 20) × 1 min/mm | 120 mm → 150 min |
Over-soaking does far less damage than under-soaking. Rapid air cooling only works below roughly 3 mm section, so forgings are water quenched.
Cold work
Cold form only from the solution-annealed condition. The work-hardening rate is well above other austenitic stainless steels, so size the press accordingly. Heavy work may need an interstage anneal, and total cold reduction past roughly 15 % should be followed by a final solution anneal.
8. Machining, welding and descaling
Machining
Machine from the solution-annealed condition. Because the alloy hardens fast under the tool, run low cutting speed with moderate feed and keep the tool engaged. A tool that dwells leaves a hardened skin the next pass has to cut through. Take enough depth of cut to get under the strain-hardened layer and flood with coolant, water-based for preference.
Welding
R20033 welds by gas tungsten arc with matching filler, by plasma arc and by laser. Practical points from shop work:
- Weld solution-annealed material only, free of scale, grease and marking media. Degrease the seam faces with acetone.
- Keep heat input low and hold interpass temperature at or below 100 °C.
- Run thin stringer beads. Nitrogen makes the weld pool prone to porosity, and thin passes let it degas.
- Open butt joints to roughly 60 to 70 degrees included with a 1 to 3 mm root gap, which allows for the low thermal conductivity and the higher expansion.
- Shield with argon and give the root clean gas backing. Post-weld heat treatment is normally not required.
Descaling and pickling
Oxide and weld heat tint cling harder than on standard stainless. Grind with fine belts or discs and avoid grinding burn. Before pickling in nitric/hydrofluoric acid, break the oxide by grit blasting, fine grinding or a salt-bath pre-treatment, then keep bath strength and temperature under control. Where access allows, brushing a weld while it is still warm removes heat tint with no pickling at all.
9. Forged product range
We are a forge with its own melt shop, not a stockist reselling mill product. R20033 runs to order: melted and refined in house, forged or ring-rolled, solution annealed, machined where the drawing calls for it, then tested before release.
| Form | Size range | Notes |
|---|---|---|
| Round bar, rod, shafts | Ø 80–1200 mm, length to 6000 mm | Turned, peeled or black. Stepped shafts to drawing. |
| Square, rectangular, flat, hex bar | Thickness 30–800 mm | Saw-cut to length |
| Seamless rolled rings | OD 200–3500 mm, wall 30–500 mm, height to 1000 mm | Rectangular or contoured section |
| Flanges | DN 15–DN 2000 (½″–80″), to Class 2500 | WN, SO, BL, LJ, orifice and specials. ASTM B462. |
| Discs, blanks, tubesheets, plates | Ø 100–2500 mm, thickness 20–600 mm | Proof-machined for volumetric inspection on request |
| Hollow bars, sleeves, bushes, cylinders | OD 120–1500 mm, ID from 60 mm | Trepanned or expanded. Bored and honed on request. |
| Blocks, valve bodies, hubs, housings, casings | To 8000 kg single piece in this grade | Open-die to drawing |
Delivery condition
- Standard: forged, solution annealed 1100 to 1150 °C, water quenched, descaled.
- Surface: black as-forged and descaled, rough machined, or finish machined to drawing tolerance.
- Machining allowance: 6 to 12 mm per side on rough-machined parts, agreed per order.
- Marking: hard stamp or low-stress vibro marking with grade, heat number, order number and specification, using sulphur-free and chloride-free media.
10. Testing and certification
| Category | Scope |
|---|---|
| Chemical analysis | Full spectro analysis per heat including N, C and S. PREN per heat on request. |
| Mechanical testing | Tensile (Rp0.2, Rp1.0, Rm, A), Brinell hardness, ISO-V impact at 20 °C or low temperature |
| Non-destructive testing | Ultrasonic, dye penetrant, dimensional inspection. Radiography on request. |
| Corrosion testing | Intergranular corrosion to ASTM A262 practice C or to customer specification |
| Heat-treatment records | Calibrated furnace charts with charge, soak and quench data for every lot |
| Certification | EN 10204 3.1 standard. EN 10204 3.2 with third-party witness (TÜV, BV, SGS, Lloyd's Register, DNV) on request. |
| Third-party inspection | Welcome at any stage. Customer-witnessed or agency-witnessed testing arranged at order. |
11. Comparison with other grades
| Grade | UNS | Cr | Ni | Mo | N | PREN | Strongest in |
|---|---|---|---|---|---|---|---|
| R20033 / Alloy 33 / 1.4591 | R20033 | 33 | 31 | 1.6 | 0.4 | 45 | Hot concentrated H2SO4, HNO3, HNO3/HF, alkalis, seawater |
| Alloy 31 / 1.4562 | N08031 | 27 | 31 | 6.5 | 0.2 | 51 | Reducing acids, phosphoric acid, mixed chloride duty |
| 254 SMO / 1.4547 | S31254 | 20 | 18 | 6.1 | 0.2 | 43 | Seawater, chloride pitting, bleach plant |
| 904L / 1.4539 | N08904 | 20 | 25 | 4.3 | – | 34 | Dilute sulphuric and phosphoric acid |
| Super duplex 2507 | S32750 | 25 | 7 | 3.8 | 0.27 | 42 | High-strength chloride duty, offshore |
| 316L / 1.4404 | S31603 | 17 | 12 | 2.2 | – | 24 | General chemical and food duty |
Where the threat is oxidising, meaning concentrated sulphuric acid at temperature, nitric acid or HNO3/HF, the 33 % chromium is what counts, and R20033 outlasts higher-molybdenum alloys even though its PREN sits below Alloy 31. Where the threat is reducing acid, a molybdenum-rich grade such as Alloy 31 or a nickel alloy usually serves better. Where chloride pitting drives the choice, R20033 and the 6 % Mo grades are close, but R20033 carries far more proof strength, which can cut wall thickness and forging weight. Final material selection for a given stream rests with the purchaser.
12. Questions and answers
What is UNS R20033?
UNS R20033 is a nitrogen-alloyed high-chromium austenitic alloy introduced in 1995. It contains nominally 33 % chromium, 31 % nickel, 32 % iron, 1.6 % molybdenum, 0.6 % copper and 0.4 % nitrogen. The same material is designated W.Nr. 1.4591, X1CrNiMoCuN33-32-1, Alloy 33 and Nicrofer 3033. It was developed for strongly oxidising service such as hot concentrated sulphuric acid, nitric acid and nitric/hydrofluoric acid mixtures, and it resists chloride pitting well despite a low molybdenum content.
Is UNS R20033 the same as Alloy 33 and 1.4591?
Yes. UNS R20033, W.Nr. 1.4591, EN name X1CrNiMoCuN33-32-1, Alloy 33 and Nicrofer 3033 all name one material. Some distributors quote UNS N08033. ASTM specifications use R20033. Our page under the European designation is 1.4591 forgings.
Which specifications cover UNS R20033?
ASTM B462 covers forged or rolled pipe flanges, forged fittings, valves and parts in UNS R20033 for corrosive high-temperature service, and governs most forgings. ASTM B649 covers bar and wire, ASTM B625 covers plate, sheet and strip, ASTM B622 covers seamless pipe and tube, and ASTM B619 covers welded pipe. VdTÜV Material Data Sheet 516 carries the European pressure-vessel data.
What are the mechanical minimums for UNS R20033?
The figures depend on which document you order against. ASTM B625 plate minimums are 87 ksi (600 MPa) tensile, 43,000 psi (295 MPa) yield at 0.2 % offset and 40 % elongation. ASTM B622 seamless pipe minimums are 750 MPa tensile and 380 MPa yield. VdTÜV 516 and the alloy producer data sheet give higher guaranteed values for solution-annealed bar and plate: Rp0.2 at least 380 MPa, Rp1.0 at least 420 MPa, Rm 720 to 920 MPa and elongation at least 40 %. Order against the document your design is based on.
What is the forging temperature for UNS R20033?
Forge between 1200 °C and 1000 °C (2192 to 1832 °F). Charge the billet into a furnace already at temperature and cool quickly after forging. Do not finish below 1000 °C, because the alloy is strong hot and work-hardens fast. A solution anneal at 1100 to 1150 °C with a water quench is needed after forging to restore corrosion resistance.
How does UNS R20033 behave in sulphuric acid?
In 98 % sulphuric acid over a seven-day laboratory test the corrosion rate is 0.04 mm/a at 100 °C, 0.07 mm/a at 125 °C, 0.08 mm/a at 150 °C, 0.16 mm/a at 175 °C and 0.04 mm/a at 200 °C. In flowing 99.1 % acid at 150 °C over 134 days the rate stayed below 0.01 mm/a, and in flowing 96 to 98.5 % acid at 135 to 140 °C over 14 days it was also below 0.01 mm/a. Performance depends on the surface being clean and metallically bright in service.
Can UNS R20033 be welded?
Yes. UNS R20033 is welded by gas tungsten arc welding with a matching filler, by plasma arc welding and by laser welding. A matching weld deposit reaches mechanical properties and impact toughness close to the wrought material, with no measured toughness loss in the heat-affected zone. Weld only solution-annealed, degreased material, keep heat input low and use thin stringer beads, since the nitrogen content makes the weld pool prone to porosity.
Does Jiangyin Jiangnan Metal stock UNS R20033?
UNS R20033 is forged to order rather than held as shelf stock. We melt and forge it in one works, solution anneal it in house and test it before release. Normal lead time is 25 to 40 days depending on size and test scope. Send a drawing, or the dimensions, quantity, specification and test requirements, to sales@steelforgepieces.com.
What certification comes with UNS R20033 forgings?
EN 10204 3.1 certificates are standard and cover heat chemistry, mechanical properties, heat-treatment records and NDT results. EN 10204 3.2 certificates witnessed by a third party such as TÜV, BV, SGS, Lloyd's Register or DNV can be arranged at order stage, as can customer-witnessed inspection.
Ask for a price on UNS R20033 forgings
Send a drawing, or just the form, dimensions, quantity and specification. You get weight, lead time and price back within one working day.
Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel 0086-189-2135-9659 · Email sales@steelforgepieces.com
Citing this page
This page may be quoted as a technical reference for UNS R20033 / Alloy 33 / 1.4591, with attribution.
Jiangyin Jiangnan Metal Co., Ltd. (2026). UNS R20033 Forgings: Alloy 33 / 1.4591 Bars, Rolled Rings, Flanges and Discs. Jiangyin, Jiangsu, China. https://www.steelforgepieces.com/Stainless-Steel/UNS-R20033.html
A plain-text version of this page is at UNS-R20033.md.
References
- ASTM B462, Standard Specification for Forged or Rolled Nickel Alloy and UNS R20033 Pipe Flanges, Forged Fittings, and Valves and Parts for Corrosive High-Temperature Service.
- ASTM B649, Standard Specification for Ni-Fe-Cr-Mo-Cu Low-Carbon Alloys and Cr-Ni-Fe-N Low-Carbon Alloy (UNS R20033) Bar and Wire.
- ASTM B625, Standard Specification for Plate, Sheet and Strip. Plate minimums for R20033: 87 ksi (600 MPa) tensile, 43,000 psi (295 MPa) yield, 40 % elongation.
- ASTM B622 and ASTM B619, seamless and welded pipe and tube specifications covering UNS R20033.
- VdTÜV Material Data Sheet 516, approval data for 1.4591 / R20033.
- M. Köhler, U. Heubner, K.-W. Eichenhofer, M. Renner, Progress with Alloy 33 (UNS R20033), a New Corrosion-Resistant Chromium-Based Austenitic Material, CORROSION 96, Paper 428, NACE International, 1996.
- Sulphuric acid materials-of-construction technical manual, Alloy 33 data page: composition, corrosion rates in H2SO4, welding.
- Alloy producer material data sheet for Alloy 33 / Nicrofer 3033 (1.4591 / R20033): physical properties, fabrication and application data.
Data is published for engineering guidance and is not a guarantee of properties in a particular application. Where sources differ, most notably between ASTM product-specification minimums and VdTÜV 516 values, both figures are shown and labelled. Order against the document named on your drawing. Material selection for a given service environment rests with the purchaser. Trade names belong to their owners, and Jiangyin Jiangnan Metal Co., Ltd. is not affiliated with any alloy producer named here.