GRADE AISI 632 / UNS S15700 / PH15-7Mo / EN 1.4532 MELTED AND FORGED IN ONE WORKS · JIANGYIN, CHINA · SINCE 1997 +86 189 2135 9659 · sales@steelforgepieces.com
Jiangnan Metal Open-Die Forging Works · Jiangyin, China Get a quote

Precipitation hardening stainless steel

AISI 632 Forgings UNS S15700 · PH15-7Mo · 15-7 PH · EN 1.4532 · X8CrNiMoAl15-7-2

AISI 632 is a chromium-nickel-molybdenum-aluminium semi-austenitic precipitation hardening stainless steel, designated UNS S15700 and sold as PH15-7Mo. It is 17-7 PH with about 2 percent molybdenum substituted for about 2 percent chromium, which buys higher strength at room temperature and at temperature.

Jiangyin Jiangnan Metal forges the grade into rings, seamless rolled rings, flanges, bars, discs, sleeves and shafts to ASTM A564, A579 and A705 Grade 632 and AMS 5657. The steel is melted on site, so the certificate traces back to a melt number rather than to a purchased billet.

Grade summaryS15700
Designations
AISI 632, UNS S15700, PH15-7Mo, 15-7 Mo, 15-7 PH, EN 1.4532
Class
Semi-austenitic precipitation hardening stainless steel
Nominal
15 Cr, 7 Ni, 2 to 3 Mo, 1 Al, balance Fe
Forging specs
ASTM A564, A579, A705 Grade 632, ASTM A461, AMS 5657
Conditions
A annealed, TH 1050, RH 950 on enquiry
Strength
to about 1448 MPa UTS in TH 1050
Service limit
about 482 C
Melting
EF, LF, VOD. VAR or ESR remelt available
Certification
EN 10204 3.1, or 3.2 witnessed
Minimum order
10 kg, no minimum piece count
01

What the grade is for

AISI 632 earns its place where a 400-series martensitic grade would be strong enough but corrodes too readily, and an austenitic grade resists corrosion well enough but cannot carry the load.

The semi-austenitic precipitation hardening grades are specified as much for how they are processed as for what they end up at. The alloy is delivered soft and austenitic, in Condition A, where it forges and machines without difficulty. Strength comes later, from low-temperature ageing. Because there is no high-temperature quench in the hardening sequence, distortion stays low. On a 2 metre rolled ring or a 6 metre shaft, that is the difference between a part that can be finish-machined to drawing and one that has to be straightened first.

The grade has a long record in aerospace work and in spring-type components that need high strength. Material taken through vacuum arc or electroslag remelting gives further improvement in fatigue resistance, which is the usual choice for rotating and spring applications. Both remelting routes run in this works, on a 6 t vacuum arc furnace and 3 t and 6 t protective-atmosphere electroslag furnaces.

02

Chemical composition

AISI 632 / UNS S15700 composition, weight percent. Single figures are maxima.
ElementMinMaxFunction
Chromium, Cr14.0016.00Passive film, corrosion resistance
Nickel, Ni6.507.75Austenite stability in Condition A
Molybdenum, Mo2.003.00Strength, pitting resistance
Aluminium, Al0.751.50Hardening element
Carbon, C—0.09Residual
Manganese, Mn—1.00Residual
Silicon, Si—1.00Residual
Phosphorus, P—0.040Impurity
Sulphur, S—0.040Impurity
Iron, FeBalanceMatrix

Published limits for sulphur vary between sources, with 0.040 and 0.030 percent maximum both in circulation. State the governing specification on the order and the heat will be aimed at that limit. Because melting is on site, chemistry is set at the furnace rather than accepted as delivered.

Aluminium is the element that makes the grade work, and it is reactive. That single fact drives both the melting practice and the welding practice described further down.

03

Mechanical properties by condition

Typical published room-temperature properties. For information only, not specification minima.
Condition0.2% yieldTensileElongationHardnessAvailable on forgings
A, annealed380 MPa / 55 ksi896 MPa / 130 ksi30 to 35%88 HRBYes, supply and machining condition
TH 10501380 MPa / 200 ksi1448 MPa / 210 ksi7%43 to 44 HRCYes, standard hardened condition
RH 9501515 MPa / 220 ksi1690 MPa / 245 ksi6%48 HRCOn enquiry, see note below
C, cold reduced1310 MPa / 190 ksi1517 MPa / 220 ksi5%45 HRCNo, strip condition
CH 9001793 MPa / 260 ksi1828 MPa / 265 ksi2%50 HRCNo, requires cold reduction

On CH 900 and forgings. CH 900 is the highest-strength condition this alloy reaches, but it is obtained by heavy cold reduction to Condition C followed by ageing near 482 C. Cold reduction of that order is a strip-mill operation and cannot be applied to a forged ring, shaft or flange. Any quotation offering forgings in CH 900 is worth questioning. For forged product the practical ceiling is RH 950.

Elevated temperature, against 17-7 PH

Short-time elevated-temperature tensile data, Condition RH 950, typical published values.
TemperatureS15700 yieldS17700 yieldS15700 tensileS17700 tensile
21 C1515 MPa1380 MPa1690 MPa1550 MPa
149 C1415 MPa1325 MPa1570 MPa1435 MPa
316 C1225 MPa1165 MPa1415 MPa1305 MPa

Useful properties run to roughly 482 C. Past that the hardening precipitates coarsen and strength drops away, which puts the grade out of contention for sustained hotter service. For that duty the enquiry should move to nickel alloys such as Inconel 617 or Incoloy 800H.

04

Physical properties

Typical physical properties of AISI 632 / UNS S15700.
PropertyCondition ATH 1050RH 950
Density7.80 g/cm37.68 g/cm37.67 g/cm3
Modulus of elasticity—196 GPa200 GPa
Thermal conductivity at 21 C—15.1 W/m·K15.1 W/m·K
Thermal conductivity at 316 C—19.7 W/m·K19.2 W/m·K
Mean expansion, 21 to 93 C14.4 µm/m·K11.0 µm/m·K9.0 µm/m·K
Mean expansion, 21 to 316 C15.3 µm/m·K11.0 µm/m·K10.1 µm/m·K
Electrical resistivityabout 82 µΩ·cm, annealed or hardened
Magnetic responseWeakly magneticMagneticMagnetic

The density shift between Condition A and the aged conditions, and the drop in expansion coefficient, both follow from the austenite-to-martensite transformation. Allow for the dimensional change when a part is machined in Condition A and aged afterwards.

05

Heat treatment

Hardening needs three steps in order: condition the austenite, transform it to martensite, then precipitation harden. The two routes differ only in how the transformation is forced.

Condition TH 1050

Austenite conditioning near 760 C, typically held around 90 minutes, destabilises the austenite so martensite forms at about room temperature on cooling. Precipitation hardening follows near 565 C for about 90 minutes, air cooled. No sub-zero equipment is involved, which makes TH 1050 the economical and dependable route for heavy forged sections. This is the hardened condition supplied as standard.

Condition RH 950

Austenite conditioning near 955 C, then a hold near minus 73 C for about 8 hours to carry the transformation to completion, then precipitation hardening near 510 C. RH 950 gives the higher strength of the two forging conditions.

Before specifying RH 950, raise it at enquiry stage. The route needs a sub-zero hold near minus 73 C. Confirm the chamber capacity against your section size and quantity when the enquiry goes in, rather than after the order is placed, so the processing route and the delivery date are quoted against what the works will actually run. TH 1050 carries no such constraint.

Over-ageing

The precipitation reaction can be pushed past peak strength by too high a temperature or too long at temperature, and the result is lower strength, not higher. Furnace uniformity surveys and soak-time control on heavy sections decide whether a ring conforms or goes to scrap. Ageing here runs in car-bottom furnaces with chamber sizes to 8,000 by 2,000 by 2,000 mm, with charted records issued against each heat-treatment lot.

06

Corrosion resistance, machining, welding

Corrosion resistance

In the hardened conditions AISI 632 resists corrosion better than the hardenable 400-series martensitic grades, Type 410, 420 and 431 among them. Against Type 304 the published positions differ in emphasis. Some mill data describes the grade as approaching Type 304 in most media; other data describes it as not equal to Type 304. Both readings point the same way, so treat 632 as close to but not better than 304. Specify it for the combination of very high strength with moderate corrosion resistance, not as a replacement for 304, and not for aggressive chloride service where duplex or super-duplex grades belong.

Machining

Machine in Condition A wherever the tolerance scheme allows. In that condition the alloy work hardens quickly, so rigid setups, positive rake, sharp tooling and steady feed all matter. Once aged, hardness sits at 43 to 48 HRC and turning, drilling and milling become slow and tool-intensive. The normal production order is forge, anneal, rough machine with an ageing allowance, heat treat, then finish machine or grind only the features that need it.

Welding

The grade welds by conventional inert-gas methods and behaves much like 17-7 PH. Three points govern the result. Gas shielding is not optional, because the hardening response depends on aluminium and aluminium is lost readily to oxidation. The high aluminium content reduces arc penetration and promotes weld slag. The molybdenum addition raises ferrite in the deposit compared with 17-7 PH. Some sources rate the grade as harder to weld than 17-4 PH for these reasons. Where filler is needed, WP 15-7 Mo or W 17-7 PH is usually called for, and both austenite conditioning and precipitation hardening have to follow welding if the joint is to reach full strength. One thing the grade does not need is the preheat and post-weld anneal used on conventional hardenable stainless steels.

07

Specifications

Specifications covering AISI 632 / UNS S15700, by product form.
SpecificationProduct formApplies to forgings
ASTM A564 Grade 632Bars, forgings, forging stockYes, primary
ASTM A579 Grade 632ForgingsYes, primary
ASTM A705 Grade 632ForgingsYes, primary
ASTM A461Forged boltingYes
AMS 5657Bars and forgingsYes
AMS 5520Sheet, strip, plateNo
ASTM A693 Grade 632Plate, sheet, stripNo
MIL-S-8955Plate, sheet, stripNo
AMS 5812, AMS 5813Weld wireFiller metal only
EN 1.4532, X8CrNiMoAl15-7-2European designationCross-reference

A correction worth making. AISI 632 forgings are sometimes quoted and certified against ASTM B564. That is wrong. ASTM B564 covers nickel-alloy forgings and does not include UNS S15700. If a quotation or a mill certificate in your file cites B564 against AISI 632, ask for it to be reissued against A564, A579, A705 or AMS 5657. The same error appears on a number of supplier pages for this grade.

Watch the designation as well as the standard. AISI 632 is not 15-5 PH (S15500) and not 17-7 PH (S17700), though the names sit close together. Quote the UNS number on the order and the ambiguity disappears.

08

Product forms and capability

Produced to customer drawing or written specification in AISI 632 / UNS S15700:

  • Seamless rolled rings
  • Forged rings
  • Retaining rings
  • Flanges
  • Round bars
  • Discs and tube sheets
  • Sleeves and bushings
  • Shafts and spindles
  • Eccentric shafts
  • Hollow bars and cylinders
  • Valve stems and seat rings
  • Valve bodies and blocks
  • Gear blanks
  • Nozzles
  • Blocks and blanks
Working envelope. Grade-specific limits are confirmed at enquiry.
ItemLimitSet by
Seamless rolled ringsOD 50 to 6,000 mm6 m, 3 m and 1 m radial-axial ring mills
Forged shaftsto 14,000 mm turned lengthC61160 horizontal lathe; 15 m well furnace for vertical treatment
Discs, tube sheets, blocksto 5,000 mm machined diameter5,000 mm vertical lathe
Bored cylinders and hollow shaftsto 1,600 mm dia by 10,000 mmCNC deep-hole drilling machine
Single-piece weightto 30,000 kg60 t heat size, 6,300 t press
Minimum order10 kgNo minimum piece count
Lead time20 to 60 daysLonger where a remelting step is specified

Where the grade is used

The strength and distortion behaviour put AISI 632 into aerospace components and spring-type parts, which is where the alloy built its record. In process and energy equipment the same properties suit pump and plunger-pump shafts, valve stems and seat rings for ball, gate, globe, check and plug valves, flanges and tube sheets for heat exchangers and pressure vessels, and sleeves, discs and bushings for compressors and generators. For rotating or cyclically loaded parts, specify vacuum arc or electroslag remelted material and say so on the enquiry, since the remelting step affects both price and delivery.

09

Testing and certification

The steel is melted here, so chemistry is verified at the furnace instead of being carried over from a billet supplier's certificate.

In-house testing applied to AISI 632 forgings.
DisciplineEquipmentStandard
Chemical analysisSPECTROTEST TXC25 optical emission spectrometerASTM E415
Carbon and sulphurHIR-9440D infrared analyserASTM E1019
Alloy verificationX-Mwt3000TX handheld analyserPositive material identification
TensileWE-600B 600 kN, WDW-300ASTM A370, ISO 6892
ImpactJBN-300 with DWC-60 low-temperature bathASTM A370, to minus 60 C
HardnessTH140 Leeb testerASTM A956, converted per ASTM E140
UltrasonicPXUT-3300, USM35XS, CTS-22ASTM A388, EN 10228-3
Magnetic particleCYE-3AASTM E709
Grain sizeXJP-6A microscope with preparation lineASTM E112

Hardness acceptance on aged material deserves a word at order stage. Portable Leeb readings converted per ASTM E140 are adequate for process control, but where a specification calls for bench Rockwell or Brinell measurement, that is placed with an accredited third-party laboratory and the report is issued alongside the mill certificate. Corrosion testing to ASTM A262, G28 or G48 is handled the same way.

The works holds CCS, BV, DNV, LR and NK approvals. Certification is issued to EN 10204 3.1, or to EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector. Chemical analysis, tensile and hardness results, heat-treatment charts and ultrasonic reports are supplied per heat and per heat-treatment lot, traceable from the melt number through to shipment.

10

Questions we are asked

What is AISI 632 stainless steel?

A chromium-nickel-molybdenum-aluminium semi-austenitic precipitation hardening stainless steel, designated UNS S15700 and sold as PH15-7Mo or 15-7 Mo. Composition runs 14.00 to 16.00 percent chromium, 6.50 to 7.75 percent nickel, 2.00 to 3.00 percent molybdenum and 0.75 to 1.50 percent aluminium, balance iron. It is derived from 17-7 PH by substituting about 2 percent molybdenum for about 2 percent chromium, which raises strength at room temperature and at temperature.

Is AISI 632 the same as PH15-7Mo, 15-7 PH and 1.4532?

Yes, those are designations for one alloy. AISI 632 is the AISI type number, UNS S15700 the unified number, PH15-7Mo and 15-7 Mo the common trade names, and 1.4532 or X8CrNiMoAl15-7-2 the European designation. It is not 15-5 PH (S15500) and not 17-7 PH (S17700), which are different alloys with similar-looking names.

Which standard should AISI 632 forgings be ordered against?

ASTM A564 Grade 632 for bars, forgings and forging stock, ASTM A579 Grade 632 or ASTM A705 Grade 632 for forgings, ASTM A461 for forged bolting, or AMS 5657 for bars and forgings. AMS 5520 and ASTM A693 cover sheet, strip and plate and are not forging specifications. ASTM B564 is a nickel-alloy forging specification and does not cover this grade, so a certificate citing it should be reissued.

Can AISI 632 forgings be supplied in Condition CH 900?

No. CH 900 is reached by heavy cold reduction to Condition C followed by ageing near 482 C, which is a strip-processing route. For open-die forgings the available conditions are A, TH 1050 and RH 950, and RH 950 is the strongest of them at about 1515 MPa yield and 1690 MPa tensile.

How does the grade compare with 17-4 PH for forged parts?

17-4 PH is martensitic and hardens in one ageing step, so it is simpler to process and is better regarded for welding. AISI 632 is semi-austenitic, needs austenite conditioning before ageing, and reaches considerably higher strength with less distortion through heat treatment. Choose 632 when strength or distortion control decides the part, and 17-4 PH when fabrication and welding decide it.

What is the maximum service temperature?

Roughly 482 C for useful mechanical properties. In Condition RH 950 at 316 C the grade still shows about 1225 MPa yield strength. Above about 482 C the hardening precipitates coarsen and strength falls, so the selection should move to a different alloy family.

What size and weight can you forge in this grade?

Rings roll to 6,000 mm outside diameter and down to 50 mm by the upset-and-punch route. The heaviest single forging is 30 tonnes, worked on 6,300 t, 4,000 t and 2,000 t presses. Shafts turn to 14,000 mm, discs to 5,000 mm diameter. Minimum order is 10 kg with no minimum piece count. Grade-specific limits depend on section size and the heat treatment specified, so send the drawing and they will be confirmed against the quotation.

How long does an AISI 632 forging take?

20 to 60 days from order confirmation. Standard melting through the electric arc furnace with ladle refining and vacuum decarburisation sits at the lower end. Specifying vacuum arc or electroslag remelted material, witnessed inspection to EN 10204 3.2, or testing placed with an outside laboratory moves the date out, so flag all three at enquiry stage to have them built into the quoted delivery rather than added afterwards.

11

Request a quotation

Send the grade or specification, the dimensions or a drawing in PDF, DWG, DXF or STEP, the quantity, the delivery condition, the heat treatment and testing requirements and the destination port. A complete enquiry is normally priced within two working days.

Jiangyin Jiangnan Metal Co., Ltd.
Open-die forging factory and integrated melting works, established 1997
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, 214423
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Hours: Monday to Saturday, 08:00 to 17:30 China Standard Time, UTC+8