Jiangyin Jiangnan Metal Co., Ltd. | Open-Die Forging Factory · Jiangsu, China · Est. 1997 | +86 189 2135 9659 | sales@steelforgepieces.com
Jiangnan Metal Melting · Open-die forging · Ring rolling

Austenitic stainless steel · Grade datasheet & forging capability

1.4438 Forgings in X2CrNiMo18-15-4

EN number 1.4438 · EN name X2CrNiMo18-15-4 · nearest UNS S31703 / AISI 317L · ASTM A182 F317L

Jiangyin Jiangnan Metal Co., Ltd. melts and open-die forges 1.4438 stainless steel in one works in Jiangyin, Jiangsu, China. 1.4438 is a low-carbon, 3–4 % molybdenum austenitic stainless steel with a higher nickel content than 316L, used where chloride pitting and crevice corrosion outrun the 316L family. We supply it as seamless rolled rings to 6,000 mm outside diameter, flanges, shafts, discs, tube sheets, sleeves and bars, in single pieces up to 30 tonnes, with EN 10204 3.1 or 3.2 certification.

EN number
1.4438
EN name
X2CrNiMo18-15-4
Nearest UNS
S31703 (317L)
PREN
≈ 27 – 34
Max ring OD
6,000 mm
Max single piece
30,000 kg
Minimum order
10 kg
Lead time
20 – 60 days
§ 01

What 1.4438 is, and when it is specified

1.4438 (X2CrNiMo18-15-4) is a low-carbon austenitic stainless steel containing 17.5–19.5 % chromium, 13.0–16.0 % nickel and 3.0–4.0 % molybdenum. It sits one step above 316L / 1.4404 in the austenitic range: the molybdenum content is raised from 2–3 % to 3–4 % and the nickel floor is raised to 13 %, which improves resistance to chloride pitting, crevice corrosion and sulphuric and phosphoric acid service while keeping the low carbon content that prevents sensitisation during welding.

The grade is specified under EN 10088-2 (sheet and plate) and EN 10088-3 (semi-finished products, bars, rods and sections), and is the European counterpart of the AISI 317L family. In pressure equipment it is usually ordered against ASTM A182 F317L or UNS S31703 when the drawing follows ASME practice, and against 1.4438 when the drawing follows EN practice. The two are close but not interchangeable without checking the nickel range. See section 04.

Jiangyin Jiangnan Metal forges 1.4438 for customers in chemical processing, flue-gas desulphurisation, pulp and paper, offshore oil and gas, seawater handling and pharmaceutical plant. Because the steel is melted on site rather than bought in as billet, the chemistry can be aimed at the forging it will become, and the mill certificate traces the part back to its melt number instead of stopping at a purchased billet.

Where 1.4438 earns its cost over 316L

  • Chloride pitting. The extra molybdenum raises the pitting resistance equivalent number by roughly 6 points over 316L, which moves the critical pitting temperature up by a useful margin in warm chloride-bearing process streams.
  • Sulphuric and phosphoric acid. 317L-type chemistry is a standard choice for dilute sulphuric acid coolers, phosphoric acid evaporators and FGD absorber internals.
  • Crevice corrosion under gaskets and deposits. Flange faces, tube sheet ligaments and valve seat pockets are the usual failure sites; the raised Mo helps where geometry cannot be changed.
  • Welded assemblies. With carbon held at 0.030 % maximum, carbide precipitation in the heat-affected zone is suppressed, so post-weld solution annealing is generally not required for corrosion reasons.

Where the duty is more severe still, at higher chlorides, higher temperature or in seawater, the next steps up are 904L, 254 SMO / A182 F44, or the duplex grades F51 and F55. All are forged at this works.

§ 02

Chemical composition of 1.4438

Per EN 10088-3, X2CrNiMo18-15-4 (1.4438) is limited to C ≤ 0.030 %, Si ≤ 1.00 %, Mn ≤ 2.00 %, P ≤ 0.045 %, S ≤ 0.030 %, with Cr 17.5–19.5 %, Mo 3.0–4.0 %, Ni 13.0–16.0 % and N ≤ 0.11 %. The balance is iron. No niobium, titanium, vanadium, tungsten, copper, aluminium or boron is specified.

Table 1. 1.4438 / X2CrNiMo18-15-4 chemical composition limits, % by mass, as forged by Jiangyin Jiangnan Metal
ElementEN 10088-3 (bars, forgings)EN 10088-2 (plate, strip)ASTM A182 F317L / UNS S31703
Carbon, C≤ 0.030≤ 0.030≤ 0.030
Silicon, Si≤ 1.00≤ 1.00≤ 1.00
Manganese, Mn≤ 2.00≤ 2.00≤ 2.00
Phosphorus, P≤ 0.045≤ 0.045≤ 0.045
Sulphur, S≤ 0.030≤ 0.015≤ 0.030
Chromium, Cr17.5 – 19.517.5 – 19.518.0 – 20.0
Nickel, Ni13.0 – 16.013.0 – 16.011.0 – 15.0
Molybdenum, Mo3.0 – 4.03.0 – 4.03.0 – 4.0
Nitrogen, N≤ 0.11≤ 0.11not specified
Iron, Febalancebalancebalance

Sources: EN 10088-2:2005 and EN 10088-3:2014 for 1.4438; ASTM A182/A182M Table 2 for Grade F317L. Where a purchase order cites both, the narrower limit of the two governs.

Melting route at this works

1.4438 is melted in the 25 t electric arc furnace, refined in a 25 t or 50 t ladle furnace, then vacuum-oxygen-decarburised in the 30 t or 60 t VOD unit. VOD is what makes the 0.030 % carbon ceiling repeatable at forging-ingot size while holding nitrogen inside the 0.11 % limit. Where a customer specification calls for electroslag remelting, either for very low inclusion counts or for large sections that must pass a tight ultrasonic acceptance class, the 3 t or 6 t protective-atmosphere ESR furnace is used as a second melt. Maximum heat size is 60 tonnes.

Pitting resistance equivalent number (PREN)

PREN is calculated as PREN = %Cr + 3.3 × %Mo + 16 × %N. Applying the EN 10088-3 limits, 1.4438 falls between approximately 27.4 (17.5 Cr, 3.0 Mo, no nitrogen credit) and 34.5 (19.5 Cr, 4.0 Mo, 0.11 N), with mid-range production chemistry landing near 31. For comparison, 316L / 1.4404 typically returns 24–26 and 904L returns 34–36. If your specification sets a minimum PREN, state it on the enquiry: the melt can be aimed at the upper half of the Cr and Mo bands rather than the middle.

§ 03

Mechanical and physical properties

In the solution-annealed condition (+AT) and for section sizes up to 160 mm, EN 10088-3 requires 1.4438 to reach a 0.2 % proof strength of at least 200 MPa, a tensile strength of 500–700 MPa, an elongation of at least 40 % longitudinal, and Charpy V-notch impact energy of at least 100 J longitudinal at room temperature. ASTM A182 F317L sets a lower bar: 485 MPa tensile minimum, 170 MPa yield minimum, 30 % elongation and 50 % reduction of area.

Table 2. 1.4438 mechanical requirements, solution annealed, room temperature
PropertyEN 10088-3, +AT, d ≤ 160 mmASTM A182 F317L
0.2 % proof strength, Rp0.2≥ 200 MPa≥ 170 MPa (25 ksi)
Tensile strength, Rm500 – 700 MPa≥ 485 MPa (70 ksi)
Elongation, A≥ 40 % (long.)≥ 30 % in 50 mm
Reduction of area, Znot specified≥ 50 %
Impact energy, KV≥ 100 J (long.)by agreement
Hardnessnot a specification requirement; typically 150–190 HB as annealednot specified for F317L

Sources: EN 10088-3:2014 for 1.4438 in the +AT condition; ASTM A182/A182M Table 3 for F317L. Values for sections heavier than 160 mm are agreed at enquiry stage. Ask for the heavy-section proposal before placing the order.

Table 3. 1.4438 typical physical properties at 20 °C
PropertyTypical value
Density7.9 – 8.0 g/cm³
Modulus of elasticity200 GPa
Thermal conductivity≈ 14 W/(m·K)
Specific heat capacity≈ 470 J/(kg·K)
Coefficient of thermal expansion, 20–100 °C≈ 16 × 10⁻⁶ /K
Magnetic responsenon-magnetic when fully annealed; slight response after cold work

Physical property values are typical for the grade and are given for design guidance. They are not certified values and are not part of the acceptance criteria on a mill certificate.

§ 04

Equivalents, cross-references and the 317L question

1.4438 is the nearest EN equivalent to AISI 317L / UNS S31703, but the two chemistries are not identical. 1.4438 requires nickel between 13.0 % and 16.0 %; UNS S31703 allows 11.0 % to 15.0 %. A heat that meets S31703 at 11.5 % nickel does not meet 1.4438. To satisfy both marks on one certificate the melt must sit in the overlap: nickel 13.0–15.0 %, chromium 18.0–19.5 %, molybdenum 3.0–4.0 %, carbon ≤ 0.030 %. Jiangyin Jiangnan Metal melts to that overlap window whenever a dual-certified 1.4438 / S31703 forging is ordered.

Table 4. 1.4438 cross-reference to other national designations
SystemDesignationRelationship
EN / DIN number1.4438the grade itself
EN / DIN nameX2CrNiMo18-15-4the grade itself
AISI / ASTM type317Lnearest equivalent; nickel band differs
UNSS31703nearest equivalent; nickel band differs
ASTM forging gradeA182 F317Lthe forging specification usually ordered against S31703
ASTM plateA240 317Lplate counterpart
ISOX2CrNiMo18-15-4same designation as EN
China GB022Cr19Ni13Mo3 / 00Cr19Ni13Mo3close equivalent
Japan JISSUS 317Lclose equivalent

Cross-reference table for guidance only. Equivalence is never exact between standards. Always state on the purchase order which specification governs acceptance, and whether dual certification is required.

1.4438 against its neighbours

Table 5. nominal comparison of 1.4438 with adjacent austenitic grades forged at this works
GradeCr %Ni %Mo %Typical PRENUsual reason to choose it
316L / 1.440416.5–18.510.0–13.02.0–2.524–26general corrosion service, lowest cost of the Mo grades
1.4438 / 317L17.5–19.513.0–16.03.0–4.0≈ 31warm chlorides, dilute sulphuric and phosphoric acid, FGD
904L / 1.453919.0–21.024.0–26.04.0–5.034–36stronger acid service, copper addition for reducing acids
254 SMO / F4419.5–20.517.5–18.56.0–6.542–45seawater and high-chloride duty
F51 / 2205 duplex21.0–23.04.5–6.52.5–3.534–36double the yield strength, chloride SCC resistance

Composition bands are nominal, drawn from the governing standard for each grade, and are shown to place 1.4438 in context rather than to specify the neighbouring grades.

Two points worth flagging before a substitution is made. First, 1.4438 is an austenitic grade: its proof strength is around 200–220 MPa, roughly a third of a 2205 duplex forging, so swapping to duplex to gain corrosion resistance usually allows a thinner section, while swapping the other way does not. Second, austenitic grades in this family remain susceptible to chloride stress corrosion cracking above roughly 60 °C; raising molybdenum improves pitting resistance but does little for SCC. Where SCC is the governing risk, duplex or a high-nickel alloy is the correct answer, not 317L.

§ 05

Forging and heat treatment practice for 1.4438

1.4438 is forged from about 1,150–1,200 °C and finished above 950 °C, then solution annealed and water quenched. ASTM A182 requires F317L to be solution treated at a minimum of 1,040 °C and liquid-quenched to below 260 °C; typical practice for 1.4438 is 1,040–1,120 °C followed by a water quench fast enough to carry the section through the 850–550 °C range without precipitating chromium carbides or sigma phase.

Why the quench rate matters on heavy sections

The 3–4 % molybdenum that makes 1.4438 useful also makes it more willing to form sigma phase than 316L if the cooling curve lingers between roughly 850 °C and 550 °C. On a 300 mm tube sheet or a heavy-section ring the core cools far more slowly than the surface, so the quench has to be designed rather than assumed: adequate tank volume, agitation, minimum delay from furnace to water, and where necessary a proof-machined section to reduce the mass being quenched. This is one of the practical reasons heavy 1.4438 forgings are worth ordering from a works that heat-treats on site instead of subcontracting it.

Equipment used for 1.4438 at this works

MELT

EF + LF + VOD

25 t electric arc furnace, 25 t and 50 t ladle furnaces, 30 t and 60 t vacuum oxygen decarburisation. Maximum heat 60 t. ESR available as a second melt where the specification calls for it.

FORGE

6,300 t press · 6 m ring mill

Hydraulic open-die presses at 6,300 t, 4,000 t and 2,000 t. Radial-axial ring rolling mills at 6 m, 3 m and 1 m. Hammers from 750 kg to 5 t for drawing out and small batch work.

HEAT TREAT

14 furnaces

Car-bottom furnaces to 8,000 × 2,000 × 2,000 mm, three high-temperature car-bottom furnaces, and two 15 m well-type furnaces that let long shafts be quenched vertically without distortion.

MACHINE

Ø5,000 mm vertical lathe

Vertical turning to Ø5,000 mm swing, horizontal lathes to 14,000 mm between centres, CNC deep-hole drilling to Ø1,600 × 10,000 mm. Proof machining for volumetric inspection is routine.

Machining and fabrication notes

  • Machining. Like other 317L-type steels, 1.4438 work-hardens readily. Use low surface speeds, a constant positive feed, rigid setups and sharp tooling; the chip is long and stringy, so chip breakers pay for themselves. Expect machinability below 304 and roughly comparable to 316L.
  • Welding. Readily welded by the usual austenitic processes. Matching or over-alloyed filler is the normal choice: 317L, or a 625-type where the weld metal has to match the parent PREN. With C ≤ 0.030 % a post-weld solution anneal is not needed to restore corrosion resistance on thin sections.
  • Hot working limits. Do not finish below about 950 °C. Heavy reductions below that temperature raise the risk of edge cracking and leave residual stress that the solution anneal then has to relieve.
  • Delivery condition. As-forged with allowance, proof-machined for ultrasonic testing, or finish-machined to drawing. State which you need in the enquiry, because it changes both the price and the inspection sequence.
§ 06

1.4438 forged product forms and size envelope

Jiangyin Jiangnan Metal supplies 1.4438 as seamless rolled rings up to 6,000 mm outside diameter, forged rings, flanges, shafts up to 14,000 mm turned length, discs and tube sheets up to Ø5,000 mm machined, bars, blocks, sleeves, bushings, bored cylinders, valve bodies and wellhead parts. The heaviest single piece is 30 tonnes; the smallest order is 10 kg, with no minimum piece count.

Table 6. 1.4438 working envelope by product form
Product formSize limitSet by
Seamless rolled ringsOD 50 mm to 6,000 mm6 m radial-axial ring mill; upset-and-punch route below mill range
Forged ringssections outside the ring-mill envelope6,300 t press, upset and punch
Forged flangesASME B16.5, B16.47 Series A/B, API 6Apress and ring mill; machined on vertical lathes
Forged shafts and spindlesup to 14,000 mm turned lengthC61160 horizontal lathe; 15 m well furnace for vertical quench
Discs, tube sheets, coversup to Ø5,000 mm machinedØ5,000 mm vertical turning lathe
Bars, blocks, billetsround, flat and square; blocks to press capacity6,300 t / 4,000 t / 2,000 t presses
Cylinders, sleeves, bushingsbored to Ø1,600 × 10,000 mmCNC deep-hole drilling machine
Valve and wellhead partsbodies, bonnets, stems, seat rings, spools, nozzlespress and machine shop; NACE MR0175 on request
Single-piece weightup to 30,000 kg60 t maximum heat size; 6,300 t press

Envelope values are plant capability limits for the grade. The practical limit on any given part is set by the most restrictive of forging, heat treatment and machining. Ask for confirmation against your drawing.

Typical applications for 1.4438 forgings

Chemical & petrochemical

Pressure-vessel flanges, tube sheets, covers, pump and valve bodies, nozzles and manifolds in dilute sulphuric and phosphoric acid service.

Flue-gas desulphurisation

Absorber internals, spray header components, damper shafts and ducting hardware where warm chloride-bearing scrubber liquor attacks 316L.

Pulp & paper

Digester and bleach-plant hardware, washer shafts, valve parts and flanges in chloride dioxide and sulphite environments.

Oil, gas & offshore

Valve bodies, seat rings, stems, spools and sleeves for topside and subsea duty, including NACE MR0175 / ISO 15156 requirements on request.

Power generation

Heat-exchanger tube sheets, condenser hardware, casing flanges and valve components in cooling water and condensate service.

Pharmaceutical & food

Reactor and vessel flanges, agitator shafts, sleeves and bushings where the low carbon content and clean surface finish matter.

§ 07

Testing, inspection and certification

Every 1.4438 forging is released against a documented route: melt analysis, mechanical testing on a representative test piece, non-destructive examination, dimensional inspection, then certification. EN 10204 3.1 mill test certificates are issued as standard. EN 10204 3.2 certificates witnessed by BV, DNV, LR, SGS, TÜV or the customer's own inspector are available on request. The works holds CCS, BV, DNV, LR and NK classification society approvals.

Carried out in the on-site laboratory

  • Chemical analysis. Optical emission spectrometry to ASTM E415, infrared carbon/sulphur analysis to ASTM E1019, handheld PMI for positive material identification.
  • Tensile testing. 600 kN and 300 kN machines to ASTM A370 and ISO 6892.
  • Impact testing. Charpy V-notch with low-temperature bath to −60 °C, to ASTM A370.
  • Ultrasonic testing. To ASTM A388 or EN 10228-3, acceptance class by agreement.
  • Magnetic particle. To ASTM E709, where applicable on machined ferritic tooling and fixtures.
  • Metallography. Grain size to ASTM E112, microstructure check for sigma phase on heavy sections.

Placed with an accredited third-party laboratory

  • ASTM A262 Practice E or Practice B, for intergranular corrosion, the usual acceptance test for an "L" grade.
  • ASTM G48 Method A, for pitting resistance in ferric chloride.
  • ASTM G28 Method A, for intergranular attack in ferric sulphate / sulphuric acid.
  • Bench Brinell or Rockwell hardness where the specification will not accept a portable instrument.
  • Impact testing below −60 °C.

State these on the enquiry, not after the order. Third-party testing has to be scheduled before shipment or it adds weeks to the delivery date.

Traceability

Because the steel is melted on site, the certificate traces the part from its melt number through forging, heat treatment and machining to shipment. A forging shop that buys billet can only trace back to a purchased billet certificate. Heat-treatment charts, NDT reports, dimensional reports and PMI records are supplied with the certificate on request.

§ 08

How to request a quotation for 1.4438 forgings

Send a drawing or a written specification to sales@steelforgepieces.com. Quotations normally come back within two working days. Minimum order is 10 kg with no minimum piece count. Lead time for 1.4438 runs 20 to 45 days from order confirmation for the standard EF + LF + VOD route, and longer if electroslag remelting or third-party witnessed inspection is required.

Table 7. what to include in a 1.4438 request for quotation
#ItemExample
1Grade and governing specification1.4438 to EN 10088-3, dual certified to ASTM A182 F317L
2Dimensions, or a drawing (PDF, DWG, DXF, STEP)OD 1,400 × ID 1,050 × H 220 mm rolled ring
3Quantity and expected repeat volume6 pcs, about twice per year
4Delivery conditionproof-machined for UT, 6 mm allowance on all faces
5Heat treatment and testing requirementssolution annealed + water quenched; UT to EN 10228-3 class 3; ASTM A262 Practice E
6Certification and destination portEN 10204 3.2 witnessed by DNV · Rotterdam

If a minimum PREN, a maximum ferrite number, or a nickel floor above the EN limit is required, say so at item 1. These are melt-shop decisions and cannot be added once the heat is poured.

Sales & engineering

Company
Jiangyin Jiangnan Metal Co., Ltd.
Plant
No.1 Chengxiqiao Road, Zhouzhuang Town,
Jiangyin City, Jiangsu Province, China
Phone
+86 189 2135 9659
WhatsApp & WeChat on the same number
Email
sales@steelforgepieces.com
Hours
Mon – Sat, 08:00 – 17:30 China Standard Time (UTC+8)

Email a 1.4438 enquiry

Customer audits, pre-shipment inspections and third-party witness testing are welcome. Wuxi Shuofang International Airport is 30 km from the plant; Shanghai's airports are 160 km. Please arrange visits by email so an English-speaking engineer is available.

§ 09

Frequently asked questions about 1.4438

What is 1.4438 stainless steel?

1.4438 is the EN material number for X2CrNiMo18-15-4, a low-carbon austenitic stainless steel containing 17.5–19.5 % chromium, 13.0–16.0 % nickel and 3.0–4.0 % molybdenum, with carbon held to 0.030 % maximum. It is specified in EN 10088-2 and EN 10088-3 and is the European counterpart of the AISI 317L family. The raised molybdenum content gives better resistance to chloride pitting and crevice corrosion than 316L, and the low carbon content prevents carbide precipitation in welded joints.

Is 1.4438 the same as 317L or UNS S31703?

They are the nearest equivalents, but they are not identical. 1.4438 requires nickel between 13.0 % and 16.0 %, while UNS S31703 permits 11.0 % to 15.0 %, and S31703 allows chromium up to 20.0 % against 19.5 % for 1.4438. A heat that meets one does not automatically meet the other.

For a forging that must carry both marks, the melt has to sit in the overlap: nickel 13.0–15.0 %, chromium 18.0–19.5 %, molybdenum 3.0–4.0 %, carbon 0.030 % maximum. Jiangyin Jiangnan Metal aims the heat at that window whenever dual certification is ordered, but it has to be stated on the enquiry, because it is a melt-shop decision that cannot be made once the heat is poured.

What is the chemical composition of 1.4438?

Per EN 10088-3: carbon 0.030 % max, silicon 1.00 % max, manganese 2.00 % max, phosphorus 0.045 % max, sulphur 0.030 % max, chromium 17.5–19.5 %, molybdenum 3.0–4.0 %, nickel 13.0–16.0 %, nitrogen 0.11 % max, balance iron. EN 10088-2, which covers plate and strip, applies a tighter sulphur limit of 0.015 % max. No niobium, titanium, vanadium, tungsten, copper, aluminium or boron is specified for this grade.

What are the mechanical properties of 1.4438?

In the solution-annealed condition for sections up to 160 mm, EN 10088-3 requires a 0.2 % proof strength of at least 200 MPa, a tensile strength of 500–700 MPa, elongation of at least 40 % longitudinal, and Charpy V-notch impact energy of at least 100 J longitudinal. ASTM A182 F317L sets lower minima: 485 MPa tensile, 170 MPa yield, 30 % elongation and 50 % reduction of area. Typical physical properties are a density of 7.9–8.0 g/cm³ and a modulus of elasticity of 200 GPa.

What is the PREN of 1.4438, and how does it compare with 316L?

Using PREN = %Cr + 3.3 × %Mo + 16 × %N, 1.4438 falls between about 27.4 and 34.5 across the full EN composition band, with typical production chemistry landing near 31. 316L / 1.4404 typically returns 24–26, so 1.4438 gains roughly six PREN points. 904L returns 34–36 and 254 SMO returns 42–45.

PREN is a ranking index for pitting resistance, not a design value. It says nothing about chloride stress corrosion cracking, which remains a risk for all of these austenitic grades above roughly 60 °C.

What heat treatment does a 1.4438 forging need?

Solution annealing followed by a water quench. Forging starts at about 1,150–1,200 °C and finishes above 950 °C; the solution anneal then runs at 1,040–1,120 °C. ASTM A182 requires F317L to be solution treated at 1,040 °C minimum and liquid quenched to below 260 °C.

On heavy sections the quench rate is the critical variable, because the 3–4 % molybdenum makes 1.4438 more willing than 316L to form sigma phase if the core lingers between 850 °C and 550 °C. Heavy tube sheets and rings are often proof-machined before the quench to reduce the mass being cooled.

What size 1.4438 forgings can you produce?

Seamless rolled rings from 50 mm up to 6,000 mm outside diameter on the 6 m radial-axial mill, with 3 m and 1 m mills for smaller sizes. Shafts up to 14,000 mm turned length. Discs and tube sheets up to Ø5,000 mm machined. Bored cylinders to Ø1,600 × 10,000 mm. The heaviest single piece is 30 tonnes, set by the 60 t maximum heat size and the 6,300 t press.

What is the minimum order quantity and lead time for 1.4438?

Minimum order is 10 kg, with no minimum piece count, because the limit is set by weight rather than quantity. A single small part is quotable and so is a one-off large ring. Lead time for 1.4438 runs 20 to 45 days from order confirmation on the standard EF + LF + VOD route. Electroslag remelting, third-party witnessed inspection to EN 10204 3.2, or corrosion testing placed with an outside laboratory each add time and should be flagged at enquiry stage so they are built into the quoted date.

Do you melt 1.4438 yourselves, or buy in billet?

We melt it. 1.4438 runs through the 25 t electric arc furnace, a 25 t or 50 t ladle furnace, and a 30 t or 60 t vacuum oxygen decarburisation unit, which is what makes the 0.030 % carbon ceiling repeatable at forging-ingot size while holding nitrogen inside the 0.11 % limit. Protective-atmosphere electroslag remelting at 3 t and 6 t is available as a second melt where the specification calls for it. Maximum heat size is 60 tonnes.

The commercial consequence is traceability: the certificate traces a part back to its melt number rather than stopping at a purchased billet certificate, which is all most forging shops in China can offer.

What certification is supplied with 1.4438 forgings?

EN 10204 3.1 mill test certificates as standard, covering melt analysis, mechanical test results, heat treatment record and non-destructive examination. EN 10204 3.2 certificates witnessed by a classification society or a third-party inspection body such as SGS or TÜV are available on request. The works holds CCS, BV, DNV, LR and NK approvals. Intergranular corrosion testing to ASTM A262, pitting testing to ASTM G48 and intergranular attack testing to ASTM G28 are placed with an accredited third-party laboratory and reported alongside the mill certificate.

Is 1.4438 magnetic?

No, not in the solution-annealed condition. 1.4438 is a fully austenitic stainless steel and is essentially non-magnetic as delivered. Cold work such as heavy machining, straightening or forming can transform a small amount of austenite to martensite at the worked surface and produce a slight magnetic response. If a non-magnetic requirement is written into the specification with a permeability limit, state it on the enquiry so the final anneal and the machining sequence can be planned around it.

Can 1.4438 be welded without post-weld heat treatment?

Generally yes. With carbon limited to 0.030 % maximum, chromium carbide precipitation in the heat-affected zone is suppressed, so a post-weld solution anneal is not required to restore corrosion resistance on normal section thicknesses. Matching 317L filler is the usual choice; a 625-type filler is used where the weld metal has to match or exceed the parent PREN. Heavy sections, highly restrained joints, or components going into severe acid service may still call for a full solution anneal after welding, but that is a design decision for the fabricator rather than a property of the grade.