Open-die forging works · Jiangyin, Jiangsu, China · Est. 1997 | 0086-189-2135-9659 | sales@steelforgepieces.com
Jiangyin Jiangnan Metal Co., Ltd. Melting · Open-die forging · Ring rolling

Precision alloy · Fe-Ni-Mn · high thermal expansion

1.3932 / NiMn20-6 Forgings Forged bar, rings, discs, sleeves and blanks in the Fe-Ni-Mn high-expansion alloy used as the active layer of thermostatic bimetal. Open-die forged to your drawing in Jiangyin, China.

Technical data sheet · Published by Jiangyin Jiangnan Metal Co., Ltd. · First published 26 May 2013 · Last reviewed 22 September 2026 · Markdown version

Material 1.3932 is the iron-nickel-manganese alloy NiMn20-6. It runs nominally 20 % nickel and 6 to 7 % manganese with the balance iron, to SEW 385, and carries the Chinese designation Ni20Mn6. There is no chromium in it, so it is not a stainless steel and it has no corrosion resistance. What it does have is a high and almost linear coefficient of thermal expansion, close to 20 x 10⁻⁶ /°C. That is the reason it is used as the active, high-expansion component of DIN 1715 thermostatic bimetal, normally bonded to Invar 36.

W.-Nr.
1.3932
Name
NiMn20-6
China
Ni20Mn6
Nickel
19-21 %
Manganese
6.0-7.0 %
CTE 20-100 °C
~20 ppm/K
Spec
SEW 385
Email an enquiry Call +86 189 2135 9659 Jump to chemistry

Summary

1.3932 is the EN and DIN material number for NiMn20-6, an austenitic iron-nickel-manganese alloy of 19.0 to 21.0 % Ni, 6.0 to 7.0 % Mn, up to 1.0 % Si and up to 0.20 % C, balance iron, specified by SEW 385.

It is a thermostatic-bimetal component alloy. It forms the high-expansion active layer that is roll-bonded to a low-expansion passive layer, almost always Invar 36 (FeNi36, 1.3912). Heating the composite bends it, and that motion switches contacts in thermostats, motor protectors and miniature circuit breakers.

The figure that matters is a mean coefficient of thermal expansion of roughly 20 x 10⁻⁶ /°C between 20 °C and 100 °C, ten to fifteen times that of its Invar partner. The difference between the two is what produces the bending.

1.3932 is not a stainless steel. It contains no deliberate chromium, so it has no corrosion resistance and will rust in damp air like plain carbon steel. Older supplier listings that file it under stainless and describe nitric acid or seawater service are describing a different alloy.

The alloy is austenitic (face-centred cubic) with a Curie point below room temperature, so it is effectively non-magnetic at ambient temperature. Being paramagnetic is also why it shows no Invar anomaly and expands so freely.

Jiangyin Jiangnan Metal Co., Ltd., an integrated melting and open-die forging works at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, forges 1.3932 into bar, rings, discs, sleeves and blanks to customer drawings and releases them with EN 10204 3.1 or 3.2 certification. Contact sales@steelforgepieces.com or +86 189 2135 9659.

01What 1.3932 is, and what it is not

1.3932 is a precision alloy with special physical properties. It is not a structural steel and not a corrosion-resisting one. The material number says as much.

Under EN 10027-2 the digits after the decimal point put a material into a family. The range 1.36xx to 1.39xx is set aside for iron materials with special physical properties, meaning alloys bought for how they expand, conduct or behave in a magnetic field rather than for strength or corrosion resistance. 1.3932 falls in that range, next to its usual partner Invar 36 (1.3912) and the sealing alloys 1.3917 (Alloy 42) and 1.3927.

The chemistry is plain: about 20 % nickel, 6 to 7 % manganese, balance iron, with silicon and carbon held down as residuals. Nickel and manganese are both austenite stabilisers, so the structure is face-centred cubic at room temperature and stays that way. There is no hardening transformation to heat treat for. The composition is tuned for the expansion coefficient and, second to that, for electrical resistivity, since those two figures decide how a bimetal strip made from the alloy deflects and how much it self-heats when current passes through it.

A correction to older listings

Correction, including to our own earlier text

For several years this page, along with a number of other trader listings for 1.3932, described the grade as a stainless steel suitable for nitric acid coolers, seawater desalination, polythionic acid service and food processing. That text belonged to a different alloy. It has been removed.

1.3932 contains no chromium. There is no passive film, no pitting resistance and no corrosion resistance of any kind, and bare parts rust in humid air. If a drawing calls for 1.3932 in a wet or chemically aggressive duty, the drawing is most likely wrong and should be queried before material is bought.

What the alloy is good at is moving predictably when it gets hot. That property, used in a bonded strip, is the basis of a large family of thermal switches and controls. The rest of this page covers the property itself, how the material is produced, and how to buy forged stock in it.

02Designations and equivalents

Drawings reach us under all of the names below. They describe the same nominal Fe-20Ni-6Mn chemistry. We accept orders under any of them and cross-list the equivalents on the material certificate.

Table 1. 1.3932 equivalent designations and the standards that define them
System or bodyDesignationNotes
EN / DIN material number1.3932Werkstoffnummer. The safest single identifier for a purchase order
EN / DIN nameNiMn20-6Also written NiMn 20-6 and NiMn20/6
SEWSEW 385Eisenlegierungen mit besonderer Wärmeausdehnung, iron alloys with special thermal expansion. The primary chemistry specification
DIN (bimetal)DIN 1715-1Thermostat metals, technical delivery conditions. Covers the bonded composite rather than the single component
DIN (older)DIN 17151Withdrawn, still quoted on legacy drawings
ChinaNi20Mn6Standard Chinese precision-alloy designation
China (bimetal strip)GB/T 4461Thermostatic bimetal strip. Ni20Mn6 is a listed active-layer component
ASTMASTM B753Standard Specification for Thermostat Component Alloys, the closest American framework
Shop namesFe-20Ni-6Mn · FeNi20Mn6 · 20Ni-6MnInformal but common on enquiries

Standards are cited at the revisions known to us at the last page review. For procurement, reference the revision in force at the contract date, and state on the order which standard governs if more than one is named.

Naming trap

1.3932 is not 1.3952. The two numbers differ by one digit and get confused on enquiries regularly. 1.3952 is X2CrNiMoN18-14-3, a non-magnetic chromium-nickel-molybdenum austenitic stainless steel used where both corrosion resistance and low permeability are required. 1.3932 is a chromium-free Fe-Ni-Mn expansion alloy with no corrosion resistance at all. If your enquiry mentions corrosion, permeability limits or pressure-retaining service, the grade you want is probably 1.3952 or 1.3964. Tell us and we will quote the right one.

03Chemical composition of 1.3932 (NiMn20-6)

The table below is the SEW 385 baseline we work to. The chemistry is kept simple. Nickel and manganese together set the expansion coefficient and hold the structure austenitic, and everything else is held low because residuals shift the expansion curve and interfere with roll bonding.

Table 2. 1.3932 / NiMn20-6 chemical composition, weight %, to SEW 385
ElementMinMaxMetallurgical role
Nickel (Ni)19.021.0With Mn, stabilises austenite and sets the expansion coefficient and the Curie point. The controlled variable
Manganese (Mn)6.07.0Strong austenite stabiliser. Suppresses the Curie point below room temperature, which is what keeps expansion high
Silicon (Si)–1.00Deoxidiser. Excess silicon embrittles and impairs bond quality
Carbon (C)–0.20Kept low. Carbides distort the expansion curve and reduce formability
Iron (Fe)BalanceMatrix
P, S and residuals–lowSulphur causes hot shortness during forging and delamination at the bond line. Held to good melting-shop practice and reported on the certificate

Limits vary slightly between standard editions, mill practices and customer specifications. If your drawing imposes tighter limits, a narrower nickel band in particular, state them on the enquiry and we will confirm before accepting the order. Certified ladle and product analysis is issued on the EN 10204 3.1 or 3.2 certificate.

Why the nickel band matters

In the iron-nickel system the expansion coefficient changes steeply with nickel content around this composition. A drift of a few tenths of a percent moves the coefficient enough to measure, and with it the specific deflection of any bimetal made from the heat. That is why the alloy is melted under close control, why heats are kept segregated, and why the mill certificate carries more weight here than on a structural grade. If several parts of one assembly have to behave identically, specify single-heat supply on the purchase order.

How we melt it

We melt 1.3932 on site by electric arc furnace with ladle refining and vacuum oxygen decarburisation (EAF + LF + VOD), adding electroslag remelting where cleanliness or section size calls for it. Maximum heat size is 60 tonnes. Melting in house means the nickel and manganese can be aimed at the finished part, and the certificate traces the forging back to its melt number rather than stopping at a purchased billet.

04Physical properties

Table 3. 1.3932 / NiMn20-6 physical properties, annealed condition, room temperature unless stated
PropertyTypical valueConfidence
Mean CTE, 20-100 °C~20 x 10⁻⁶ /°CDesign value, the property the alloy is bought for
Mean CTE, 20-200 °C~20-21 x 10⁻⁶ /°CDesign value. The curve is close to linear across this band
Crystal structureAustenitic, face-centred cubicEstablished. No phase transformation on cooling, not hardenable by heat treatment
Magnetic behaviourParamagnetic at room temperature, Curie point below ambientEstablished in principle. Specify a limit and we will measure it
Density~8.0 g/cm³Indicative. Use for forging-weight estimation only
Electrical resistivityorder of 1 µΩ·mIndicative and heat-dependent. Measured to ASTM B63 at 24 °C when the order requires it
Modulus of elasticity~150-180 GPaIndicative. Matters mainly through the bimetal bending equations
Corrosion resistanceNone to speak of, no chromiumEstablished. Protect, plate or keep dry
Read the confidence column

Expansion coefficient, structure and magnetic state are well established for this chemistry and can be used directly in design. The values marked indicative, meaning density, resistivity and modulus, vary with heat, section size and condition, and are published here for screening only. Where any physical value is contractually important, state it on the purchase order and we will report the measured result on the material certificate rather than letting a handbook figure stand in for a test.

05Thermal expansion and why the figure is high

The alloy is paramagnetic at room temperature, and that is what lets it expand freely.

In face-centred cubic iron-nickel alloys near 36 % nickel, a magnetostrictive volume contraction works against ordinary lattice expansion and cancels most of it. That is the Invar effect, and it is why Invar 36 barely moves when heated. The effect depends on the alloy being ferromagnetic. Above the Curie point it stops and expansion returns to normal.

1.3932 sits on the other side of that line by design. Nickel is dropped to about 20 % and 6 to 7 % manganese is added, which puts the Curie temperature below room temperature. In service the alloy is already paramagnetic, so nothing cancels the lattice expansion and it expands at the full rate of an austenitic metal, around 20 x 10⁻⁶ /°C. That is roughly 1.7 times carbon steel and about fifteen times its Invar partner.

Mean coefficient of thermal expansion, 20-100 °C Bar chart. Invar 36 1.3, Alloy 42 5.3, carbon steel about 12, AISI 304 about 17, 1.3932 NiMn20-6 about 20, Mn75Ni15Cu10 about 27, all in units of 10 to the minus 6 per degree Celsius. 0510 152025 Mean CTE, 20-100 °C (x10⁻⁶ /°C) Invar 36 (1.3912) 1.3 Alloy 42 (1.3917) 5.3 Carbon steel ~12 AISI 304 stainless ~17 1.3932 · NiMn20-6 ~20 Mn75Ni15Cu10 ~27
Where 1.3932 sits. The blue bars are the low-expansion passive alloys, the orange bars the high-expansion active alloys, and the grey bars two ordinary structural materials for scale. A thermostatic bimetal works on the difference between an orange bar and a blue one. Pairing 1.3932 with Invar 36 puts roughly 18 ppm/K of mismatch across the bond line, and that mismatch is the mechanism.
Specify the temperature band

Published coefficients are mean values between room temperature and a stated upper temperature, not instantaneous values at a point. A part cycling between 80 °C and 160 °C does not see the 20 to 100 °C figure. The coefficient also shifts with cold work and residual stress, which is why the alloy is used annealed. For dimensionally critical work, ask for the measured expansion curve on the delivered heat and put the temperature band on the order.

06How 1.3932 works inside a thermostatic bimetal

A thermostatic bimetal is two metal layers, sometimes three, bonded along their whole contact face. The layer with the larger expansion coefficient is the active component, and that is where 1.3932 goes. The layer with the smaller coefficient is the passive component, normally Invar 36 at 1.8 to 4.8 x 10⁻⁶ /°C.

Heat the strip and the active side tries to grow while the passive side holds it back. The strip has nowhere to go but into an arc, curving towards the passive side. Cool it and the curvature reverses. Deflection at the free end is far larger than the length change of either layer on its own, and it repeats over millions of cycles. The effect has been used for temperature control since the eighteenth century and still is.

Thermostatic bimetal strip, cold and heated Diagram. Cold, the bonded strip is flat with the 1.3932 active layer above the Invar 36 passive layer. Heated, the strip curves downward towards the passive side and its free end deflects. Cold, flat 1.3932 active (CTE ~20) Invar 36 passive (CTE ~1.3) Heated, curves towards the passive side free-end position when cold deflection A, drives the contact
The bimetal mechanism. Deflection rises with the expansion difference between the two layers and with the square of the free length, and falls with thickness. That is why strips are long and thin, and why the active alloy's coefficient is specified so tightly.

Standard pairings and the third layer

A two-layer strip has whatever electrical resistance the two alloys happen to give it. Many applications heat the bimetal by passing current through it, and then the resistance has to match the current being switched. The usual answer is a third layer of nickel or copper between the active and passive layers, working as a shunt. Deflection stays about the same while resistivity drops by as much as an order of magnitude. Chinese grade 5J1411A, for example, is Ni20Mn6 active with a copper intermediate layer, to GB/T 4461.

Table 4. Typical layer roles in a thermostatic bimetal
LayerPurposeAlloys commonly used
Active (high expansion)Generates the motion. Marked on the convex side of the heated stripNi20Mn6 / NiMn20-6 (1.3932) · Ni22Cr3 · Mn75Ni15Cu10
Passive (low expansion)Restrains the active layer so the strip curves instead of stretchingInvar 36 (FeNi36, 1.3912) · Ni42 · Ni39
Intermediate (shunt)Sets the electrical resistivity and thermal conductivity without changing deflection muchPure nickel · copper, including oxygen-free · plain steel
What we make and what we do not

We are an open-die forging works. We supply 1.3932 in forged and machined form: bar, rings, discs, sleeves, blanks and tooling stock, melted here. We do not roll-bond or clad thermostatic bimetal strip and we do not stamp bimetal elements. Finished strip to DIN 1715 or GB/T 4461 needs a strip mill. Forged components, rolling blanks, research quantities and machined parts are what this page covers.

07Mechanical properties

1.3932 is not a strength alloy. It is austenitic, cannot be hardened by heat treatment, and in service carries very little load, since a bimetal element develops force through thermal mismatch rather than through applied stress. The mechanical figures matter mostly for handling, forging and machining.

Table 5. 1.3932 typical mechanical properties, annealed forged bar. Indicative values, not specification minima
PropertyTypicalComment
Tensile strength, Rm450-600 MPaMild-steel class. Rises substantially with cold work
Yield strength, Rp0.2180-280 MPaSize the section for load, do not select this alloy for strength
Elongation A35-50 %Ductile and readily formed in the annealed condition
Hardness, annealed130-170 HVCold-rolled strip runs far harder. Forged and annealed bar does not
Work hardeningPronouncedTypical austenitic behaviour. Affects machining more than design

Cold work raises strength and ruins the expansion accuracy. Strain from drawing, straightening or heavy machining shifts the measured coefficient away from the datasheet value, then relaxes in service and moves the part. Where the expansion figure is the reason the alloy was chosen, the sequence is forge, anneal, rough machine, stress relieve, finish machine. Do not cold work to strength.

08Forged forms and sizes we supply in 1.3932

Everything below is made to order against a drawing or a dimension list. There is no stock catalogue, since open-die forging exists so that you do not have to design around standard sizes. Most commercial use of this alloy is as thin strip for bonding, so the forged forms here cover blank supply, research quantities, machined components and tooling.

Table 6. 1.3932 / NiMn20-6 forged product forms and indicative size envelope
FormIndicative rangeRoute and typical use
Forged round bar25-400 mm dia.Cogged and turned. Machining stock, rolling-blank feedstock, test material
Forged flat bar and blocksto 2,000 mm longPressed and cut. Blanks for slitting and for laboratory work
Seamless rolled ringsOD 200-1,500 mmPierced and ring-rolled, continuous circumferential grain flow
Forged rings and sleevesOD 80-1,000 mmUpset and punched, or bored from solid, for sections outside the ring-mill envelope
Discs and blanks100-1,200 mm dia.Upset discs with radial grain flow. Rolling and stamping blanks
Hollow bar and bushingsOD 80-600 mmTrepanned or forged over a mandrel, rough or finish machined
Near-net and special shapesto drawingThermal-actuator bodies, spacers, instrument components

Ranges describe routine work rather than hard limits. The works runs 6,300 t, 4,000 t and 2,000 t presses, 6 m, 3 m and 1 m radial-axial ring mills and a 60 t maximum heat, so larger pieces are possible in principle. For a precision alloy the practical limit is usually set by how much material you want to buy. Send the drawing and we will say what we can make rather than quote something we cannot.

Supply conditions: as-forged with machining allowance, rough machined (turned and bored), or finish machined to drawing. Annealed as standard. Heat-treatment condition, surface protection and marking are agreed at order. Minimum order is 10 kg, with no minimum piece count.

09Forging, heat treatment, machining and welding

Forging

1.3932 is hot worked from approximately 1,100 to 1,180 °C, finishing above roughly 900 °C. It is single phase austenitic, so there is no transformation to work around, but two cautions apply, the same two that govern the iron-nickel family generally.

  • Heat quickly and do not soak. Long residence in a sulphur-bearing furnace atmosphere lets sulphur into the surface and causes hot shortness and surface checking. Furnaces are run clean and neutral to slightly reducing.
  • Stay away from the solidus. Overheating coarsens the grain irreversibly, and a coarse-grained precision alloy will not give consistent properties down the bar.

A forging reduction of at least 4:1 from the ingot breaks down the as-cast structure. After the final blow the piece is slow cooled and annealed. The anneal, not the forging, sets the expansion coefficient the customer will measure.

Heat treatment

Table 7. 1.3932 heat-treatment practice
OperationTemperatureTime and coolingPurpose
Full anneal850-1,000 °CAbout 30 min per 25 mm section, protective atmosphere or vacuum, air or water coolRemoves cold work, restores the datasheet expansion coefficient, softens for machining
Stress relief / stabilise300-350 °C1 to 4 h, slow coolApplied after final machining on precision parts, to lock dimensions before service

The alloy scales readily and has no chromium to protect it, so where surface condition matters the anneal is run under a protective atmosphere. Parts must be clean and free of grease before they go in, since fingerprints leave permanent marks.

Machining

Machining behaves like austenitic stainless steel. The alloy is gummy, work hardens under a rubbing tool and throws long stringy chips. The rules are the familiar ones: sharp positive-rake carbide tooling replaced at the first sign of edge rounding, short rigid setups, flood coolant, heavy positive feeds, and no dwelling in the cut, because a tool that stops feeding while still in contact glazes the surface and work hardens a layer for the next pass to fight through. Leave 2 to 4 mm of stock after roughing, stress relieve, then finish with light depths of cut.

Welding and joining

1.3932 welds by GTAW, electron beam and resistance methods with a matching Fe-Ni-Mn filler. Joint faces have to be clean, since sulphur and low melting point contamination cause cracking. Where the joint has to share the parent metal's expansion behaviour, a post-weld anneal is needed, otherwise the weld and heat affected zone expand on a different curve and the assembly distorts on cycling. In its intended use the alloy is not welded at all but roll bonded, which is a solid state cold pressure weld carried out at the strip mill.

10Where 1.3932 is used

Every application below relies on the same behaviour: a known, repeatable movement in response to a temperature change, delivered by a bimetal whose active half is this alloy.

Table 8. 1.3932 / NiMn20-6 applications by sector
SectorTypical componentsWhy this alloy
Low-voltage switchgearMiniature circuit breakers, motor protectors, overload releases, thermal cut-outsHeated directly by the load current, trips on a defined temperature rise. The highest-volume use of the alloy
Domestic appliancesIron and kettle regulators, oven and cooker thermostats, refrigerator and freezer controls, snap discsCheap, sturdy, self-contained temperature control needing no electronics or power
Automotive and e-mobilitySeat-heater controls, cooling-water and exhaust thermostats, flashers, battery-pack thermal cut-outsSurvives vibration and wide temperature swings, fails safe
Measurement and instrumentsBimetal dial thermometers, exhaust gas thermometers, spiral and helical measuring coils, temperature compensation elementsLinear deflection over a wide band with no power supply
Energy and environmental plantTime-delay switches, regulators, starters, thermal relays, over-temperature protectionLong-life repeatable actuation, millions of cycles
LightingFluorescent and energy-saving lamp starters, flasher unitsVery thin strip, fast thermal response

In forged form specifically, 1.3932 goes into rolling and stamping blanks for the strip mills that make the above, into machined bodies and spacers for thermal actuators, and into research and qualification quantities where a laboratory needs bar rather than strip.

11Limitations to design around

1.3932 is a specialist alloy with real drawbacks. Knowing them before ordering saves a rejected forging later.

Table 9. 1.3932 known limitations and the practical response
LimitationConsequencePractical response
No corrosion resistanceRusts in damp air like plain carbon steel. No chromium, so no passive filmPlate, paint, oil or keep dry. Standard export packing here is oiled and VCI wrapped. Never specify it for wet or chemical duty
Low strengthYield around 200 MPa, mild-steel classSize the section for load, or select a different alloy if strength is the driver
Expansion is process-sensitiveCold work, residual stress and heat treatment all shift the coefficientSpecify the coefficient and temperature band on the drawing. Agree the heat-treatment route before manufacture, not after
Heat-to-heat variationA few tenths of a percent of nickel moves the coefficient enough to measureSpecify single-heat supply where several parts must behave identically
Oxidation and scalingScales readily at annealing temperature, no chromium to protect the surfaceProtective-atmosphere or vacuum anneal where surface condition matters
Machining behaviourGummy, work hardening, stringy chips, short tool lifeSharp tools, flood coolant, no dwell, stress relief between roughing and finishing
Not a structural or pressure gradeNot listed in pressure-vessel or piping codes and should not be substituted into themIf the part is pressure retaining, this is the wrong alloy. Tell us the duty and we will quote a code-listed grade

121.3932 compared with neighbouring grades

If 1.3932 is not the right alloy, one of these usually is. Coefficients are approximate mean values near room temperature.

Table 10. 1.3932 against the alloys it is most often confused with or chosen against
GradeNominal compositionCTE (10⁻⁶ /°C)Choose it when
1.3932 · NiMn20-6Fe-20Ni-6Mn~20You need the high-expansion half of a bimetal pair, or a freely expanding austenitic alloy with no magnetic anomaly
Ni22Cr3Fe-22Ni-3Cr~19-20Similar deflection with some oxidation resistance from the chromium. The usual alternative active layer
Mn75Ni15Cu10Mn-Ni-Cu~27Maximum deflection is wanted and the service temperature is modest
Invar 36 · 1.3912Fe-36Ni~1.3The partner alloy. The passive layer, or any part that must not change length at all
Alloy 42 · 1.3917Fe-42Ni~5.3You are matching silicon, alumina or a hard sealing glass rather than building a bimetal
Alloy 48 · Alloy 52Fe-48Ni · Fe-51Ni8.7 · 10.0Sealing to soft and soda-lime glass
1.3952 · X2CrNiMoN18-14-3Fe-18Cr-14Ni-3Mo-N~16You actually wanted a non-magnetic stainless steel. Corrosion resistance plus controlled permeability
Nitronic 50 · 1.3964Fe-22Cr-12Ni-2Mo-N~16Non-magnetic, high strength and corrosion resistant. A structural answer rather than a thermal one

We forge all of the grades above. If you are still choosing, send the operating temperature range, the movement or tolerance you need to hold and the environment, and we will say which one we would use, including when the answer is a cheaper or more ordinary alloy than the one you asked about.

13Testing, inspection and certification

Because the steel is melted here, chemistry is verified at the furnace rather than taken from a supplier certificate. Every forging is released against a documented route: melt analysis, mechanical testing on a representative test piece, non-destructive examination, dimensional inspection, then certification.

Table 11. Standard and optional test scope for 1.3932 forgings
TestStandardIncluded
Chemical analysis, ladle and productSEW 385 · ASTM E415 (OES)Standard
Tensile testASTM A370 · EN ISO 6892-1Standard
HardnessASTM E10 / E140 · EN ISO 6506Standard
Ultrasonic examinationEN 10228-3 · SEP 1921 · ASTM A388Standard, acceptance class to order
Dimensional report and heat-treatment chartTo drawing, furnace recordStandard
Thermal expansion by dilatometryASTM E228 · ASTM E831On request. Recommended, since this is the property being bought
Electrical resistivityASTM B63, at 24 °COn request
Magnetic permeabilityTo agreed method and limitOn request
Grain size and micrographASTM E112On request
PMI verificationXRF / OESOn request

Certification. Forgings are released with an EN 10204 3.1 certificate issued against the mill heat, or EN 10204 3.2 witnessed by a third party such as TÜV, SGS, BV, Lloyd's Register or DNV when the order calls for it. The works holds CCS, BV, DNV, LR and NK classification society approvals and runs its own laboratory for chemistry, tensile, impact, hardness, ultrasonic, magnetic particle and metallographic work. Dilatometry is placed with an accredited third-party laboratory and the report issued alongside the mill certificate.

14How to specify a 1.3932 order

This grade carries one specification decision that most grades do not. The expansion requirement has to be stated explicitly, because it is the property being bought and the chemistry alone does not guarantee it. Send a drawing to sales@steelforgepieces.com with the items below and a quotation normally comes back within two working days.

  1. Grade and standard. "1.3932 / NiMn20-6 to SEW 385", or the designation your drawing uses.
  2. Drawing or dimensions. PDF, DWG, DXF or STEP, or simply OD x ID x length.
  3. Product form. Bar, ring, disc, sleeve, blank or machined part.
  4. Expansion requirement. The value, the temperature band it applies over, and whether it must be measured and certified.
  5. Single-heat requirement. State it if several pieces must behave identically.
  6. Supply condition. As-forged, rough machined or finish machined. Annealed as standard, plus a stabilising treatment if wanted.
  7. Test and certification scope. EN 10204 3.1 or 3.2, UT class, any additional tests from Table 11.
  8. Quantity, delivery terms, destination port and required date.
Table 12. Copy-ready drawing callout for 1.3932
MATERIAL1.3932 / NiMn20-6 to SEW 385 (Ni20Mn6, GB/T 4461)
CONDITIONAnnealed, protective atmosphere. Stabilise 320 °C / 2 h after final machining
EXPANSIONMean CTE 20 x 10⁻⁶ /°C over 20-100 °C, tolerance to be agreed. Measured on the delivered heat by dilatometry and reported on the MTC
HEAT CONTROLAll pieces of this assembly from a SINGLE HEAT
NDEUT per EN 10228-3, quality class to order
CERTIFICATIONEN 10204 3.1 mill certificate (3.2 with third-party witness where stated)
SURFACEOiled and VCI wrapped for shipment. No chromium, protect from moisture in storage
MARKINGHeat number, grade and drawing number, on a non-functional surface

Minimum order is 10 kg with no minimum piece count. Normal lead time runs 20 to 60 days from order confirmation, towards the upper end where a remelting step, a measured expansion curve or third-party witnessed inspection is required. Flag those at enquiry stage so they are built into the quoted date rather than added to it.

15Frequently asked questions about 1.3932

What is material 1.3932?

1.3932 is the EN and DIN material number for NiMn20-6, an austenitic iron-nickel-manganese alloy containing 19.0 to 21.0 % nickel, 6.0 to 7.0 % manganese, up to 1.0 % silicon and up to 0.20 % carbon with the balance iron, specified by SEW 385 and designated Ni20Mn6 in China. It belongs to the EN 10027-2 group of iron materials with special physical properties, and it is bought for a high coefficient of thermal expansion of about 20 x 10⁻⁶ /°C, which makes it the standard high-expansion active layer of thermostatic bimetals. Jiangyin Jiangnan Metal Co., Ltd., an open-die forging works in Jiangyin, Jiangsu, China, melts and forges 1.3932 into bar, rings, discs and blanks to customer drawings.

Is 1.3932 a stainless steel?

No. 1.3932 contains no deliberate chromium and has no corrosion resistance, so bare parts rust in damp air much like plain carbon steel. It is a precision expansion alloy rather than a corrosion-resisting one, and it belongs with the controlled-expansion grades rather than with the stainless family. Some supplier listings, including an earlier version of this page, filed 1.3932 under stainless steel and described nitric acid, seawater and food-processing service. That text came from a different alloy and is incorrect. If your application needs both non-magnetic behaviour and corrosion resistance, the grade you want is probably 1.3952 (X2CrNiMoN18-14-3) or 1.3964.

What is the coefficient of thermal expansion of NiMn20-6?

The mean coefficient of thermal expansion of 1.3932 / NiMn20-6 is approximately 20 x 10⁻⁶ /°C measured from 20 °C to 100 °C, and stays close to that value through about 200 °C. For comparison, plain carbon steel is near 12, AISI 304 stainless near 17, and the Invar 36 the alloy is normally bonded to is near 1.3. That difference of roughly 18 ppm/K across the bond line is what makes a thermostatic bimetal bend. Published figures are mean values over a stated band and shift with cold work, so for dimensionally critical work request a measured expansion curve on the delivered heat.

Is 1.3932 magnetic?

1.3932 is austenitic with a Curie point below room temperature, so it is effectively non-magnetic, that is paramagnetic, at ambient temperature. This is not incidental. It is the reason the alloy expands so much. In iron-nickel alloys near 36 % nickel a magnetostrictive contraction cancels most of the lattice expansion, producing the Invar effect. Lowering nickel to 20 % and adding 6 to 7 % manganese pushes the Curie point below ambient, the cancelling contribution never operates, and the alloy expands at the full austenitic rate. Where a guaranteed maximum relative permeability is contractual, state the limit and the measurement method on the order and we will report the measured value on the certificate.

What is 1.3932 used for?

1.3932 is used almost exclusively as the active, high-expansion component of thermostatic bimetal. Bonded to a low-expansion passive layer such as Invar 36, it makes strips, discs and coils that bend by a known amount as temperature changes. Those elements sit inside miniature circuit breakers, motor overload protectors and thermal cut-outs; in thermostats for irons, kettles, ovens, refrigerators and cooking appliances; in automotive cooling-water, exhaust and seat-heater controls; in bimetal dial and exhaust gas thermometers and temperature compensation elements; and in fluorescent lamp starters, flashers and time-delay switches. In forged form specifically it is supplied as rolling and stamping blanks, machined actuator components and research quantities.

What standards cover 1.3932 / NiMn20-6?

The chemistry is specified by SEW 385, the Stahl-Eisen-Werkstoffblatt for iron alloys with special thermal expansion. The bonded thermostatic bimetal composite that uses it is covered by DIN 1715-1 in Germany and by GB/T 4461 in China, where the alloy is designated Ni20Mn6. ASTM B753 is the closest American framework for thermostat component alloys. The older DIN 17151 is sometimes quoted on legacy drawings. We accept orders under any of these designations and cross-list the equivalents on the EN 10204 certificate.

Can 1.3932 be forged, and at what temperature?

Yes. 1.3932 is hot worked from approximately 1,100 to 1,180 °C with the finishing temperature held above roughly 900 °C. The alloy is single phase austenitic, so there is no transformation to work around, but it should be heated quickly rather than soaked. Prolonged residence in a sulphur-bearing furnace atmosphere causes hot shortness and surface checking, and overheating near the solidus coarsens the grain irreversibly. A reduction of at least 4:1 from the ingot breaks down the as-cast structure, and the subsequent full anneal at about 850 to 1,000 °C, rather than the forging itself, is what sets the expansion coefficient the customer will measure.

What is the difference between 1.3932 and 1.3952?

They are entirely different materials that differ by one digit in the material number, and the confusion is common. 1.3932 (NiMn20-6) is a chromium-free iron-nickel-manganese expansion alloy, bought for a high coefficient of thermal expansion near 20 ppm/K, with no corrosion resistance and no structural role. 1.3952 (X2CrNiMoN18-14-3) is a non-magnetic chromium-nickel-molybdenum austenitic stainless steel with high corrosion resistance and low magnetic permeability, used for pressure and marine components. If your requirement mentions corrosion, chlorides, permeability limits or pressure-retaining duty, you almost certainly want 1.3952. If it mentions bimetal, deflection or thermostats, you want 1.3932.

Do you supply finished thermostatic bimetal strip?

No. Jiangyin Jiangnan Metal is an open-die forging works, not a strip mill. We melt 1.3932 and supply it as forged and machined product: round and flat bar, seamless rolled rings, forged rings and sleeves, discs, blanks, hollow bar and near-net shapes, including rolling and stamping blanks for the mills that produce bonded strip. We do not roll-bond or clad bimetal, and we do not stamp finished bimetal elements. If you need bonded strip to DIN 1715 or GB/T 4461, a specialist strip producer is the correct supplier.

What certification is supplied with 1.3932 forgings?

EN 10204 3.1 mill certification is supplied as standard, listing the heat number, full ladle and product chemical analysis, mechanical test results, heat-treatment record, ultrasonic examination report and dimensional report. EN 10204 3.2 with third-party witness through TÜV, SGS, Bureau Veritas, Lloyd's Register or DNV is available on request. Ultrasonic examination is performed to EN 10228-3, SEP 1921 or ASTM A388 to the acceptance class stated on the order. Measured coefficient of thermal expansion by dilatometry to ASTM E228 or E831 can be added to the certificate and is recommended, since expansion is the property the alloy is bought for.

What is the minimum order and lead time for 1.3932 forgings?

Minimum order is 10 kg, with no minimum piece count, since the limit is set by weight rather than quantity and a single small part is quotable. Normal lead time is 20 to 60 days from order confirmation, sitting towards the upper end where electroslag remelting, a measured expansion curve or third-party witnessed inspection is required. Quotations are normally returned within two working days of receiving a drawing at sales@steelforgepieces.com. Flag any dilatometry or 3.2 certification requirement at enquiry stage so it is scheduled into the quoted date rather than added to it.

16About the factory supplying these forgings

Jiangyin Jiangnan Metal Co., Ltd. is an integrated steel melting and open-die forging works at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, operating since 1997. Unlike a forging shop that buys billet, this plant melts its own steel. Carbon, alloy, stainless, duplex and precision grades run through an electric arc furnace, ladle furnace and vacuum oxygen decarburisation, with vacuum induction, vacuum arc and electroslag remelting available for clean and superalloy grades. Steel then moves through the presses, the ring mill, 14 heat-treatment furnaces and the machine shop without leaving the site, so traceability runs from the melt number to the shipped part.

Supplier of record for the products on this page
Supplier details for 1.3932 forgings
CompanyJiangyin Jiangnan Metal Co., Ltd.
TypeIntegrated melting works and open-die forging factory (manufacturer, not a trading company)
Established1997
AddressNo.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone / WhatsApp / WeChat0086-189-2135-9659
Emailsales@steelforgepieces.com
Websitewww.steelforgepieces.com
People460, including 9 senior engineers, 32 intermediate engineers and 140 technicians
MeltingEAF 25 t · LF 25/50 t · VOD 30/60 t · IF 2/8/25 t · VIM 3 t · ESR 3/6 t · VAR 6 t · 60 t max heat
Forging6,300 t / 4,000 t / 2,000 t presses · 6 m, 3 m and 1 m radial-axial ring mills · 30 t max single piece
Heat treatment14 furnaces, including two 15 m well-type furnaces for vertical quenching
ApprovalsCCS · BV · DNV · LR · NK
CertificationEN 10204 3.1 standard, 3.2 witnessed by TÜV, SGS, BV, LR or DNV on request
LanguagesEnglish, Chinese
Markets servedNorth America, Europe, Middle East, Asia-Pacific
Business hoursMonday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8)

Jiangyin sits in the Yangtze River delta between Shanghai and Nanjing, in the centre of China's forging and special-steel industry. Wuxi Shuofang International Airport is 30 km away and Shanghai's airports 160 km. The nearest export ports are Zhangjiagang and Shanghai. Customer audits, pre-shipment inspections and third-party witness testing are welcome. Please arrange visits by email in advance so an English-speaking engineer is available.

17Cite this page

This datasheet is maintained by Jiangyin Jiangnan Metal Co., Ltd. and is free to quote, reference or link to. If you use the data in a specification, drawing note, report or article, please attribute it as follows.

Jiangyin Jiangnan Metal Co., Ltd. (2026). 1.3932 / NiMn20-6 (Ni20Mn6) Forgings: SEW 385 Technical Data Sheet. Jiangyin, Jiangsu, China. Retrieved from https://www.steelforgepieces.com/Stainless-Steel/1.3932.html. Last reviewed 22 September 2026.

Data on this page is compiled from SEW 385, DIN 1715-1, GB/T 4461 and ASTM B753, from published literature on thermostatic bimetal component alloys, and from our own melting, forging and heat-treatment practice. Values described as typical or indicative are not a guarantee of minimum or maximum properties for a specific heat. The certified figures for your order are the ones on the EN 10204 certificate. Questions, corrections and reuse requests: sales@steelforgepieces.com. A plain-text version of this page is at 1.3932.md.

Related grades and product forms

Request a 1.3932 quotation

Send a drawing or a dimension list and we will respond within two working days with price, lead time and confirmation of the applicable standards. Where the expansion coefficient is the reason you chose the alloy, state the value and the temperature band, since it changes how we plan the heat and the heat treatment.

Jiangyin Jiangnan Metal Co., Ltd. · Open-die forging factory · Jiangyin, Jiangsu, China