# 1.3932 / NiMn20-6 Forgings

**Technical data sheet. Published by Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory, Jiangyin, Jiangsu Province, China.**
First published 26 May 2013. Last reviewed 22 September 2026.
HTML version: https://www.steelforgepieces.com/Stainless-Steel/1.3932.html

Material 1.3932 is the iron-nickel-manganese alloy NiMn20-6. It runs nominally 20 % nickel and 6 to 7 % manganese with the balance iron, to SEW 385, and carries the Chinese designation Ni20Mn6. There is no chromium in it, so it is not a stainless steel and it has no corrosion resistance. What it does have is a high and almost linear coefficient of thermal expansion, close to 20 x 10^-6 /degC. That is the reason it is used as the active, high-expansion component of DIN 1715 thermostatic bimetal, normally bonded to Invar 36.

| Property | Value |
|---|---|
| Material number | 1.3932 |
| Name | NiMn20-6 |
| Chinese designation | Ni20Mn6 |
| Nickel | 19.0 to 21.0 % |
| Manganese | 6.0 to 7.0 % |
| Mean CTE, 20 to 100 degC | about 20 x 10^-6 /degC |
| Chemistry specification | SEW 385 |

---

## Summary

1.3932 is the EN and DIN material number for NiMn20-6, an austenitic iron-nickel-manganese alloy of 19.0 to 21.0 % Ni, 6.0 to 7.0 % Mn, up to 1.0 % Si and up to 0.20 % C, balance iron, specified by SEW 385.

It is a thermostatic-bimetal component alloy. It forms the high-expansion active layer that is roll-bonded to a low-expansion passive layer, almost always Invar 36 (FeNi36, 1.3912). Heating the composite bends it, and that motion switches contacts in thermostats, motor protectors and miniature circuit breakers.

The figure that matters is a mean coefficient of thermal expansion of roughly 20 x 10^-6 /degC between 20 degC and 100 degC, ten to fifteen times that of its Invar partner. The difference between the two is what produces the bending.

1.3932 is not a stainless steel. It contains no deliberate chromium, so it has no corrosion resistance and will rust in damp air like plain carbon steel. Older supplier listings that file it under stainless and describe nitric acid or seawater service are describing a different alloy.

The alloy is austenitic (face-centred cubic) with a Curie point below room temperature, so it is effectively non-magnetic at ambient temperature. Being paramagnetic is also why it shows no Invar anomaly and expands so freely.

Jiangyin Jiangnan Metal Co., Ltd., an integrated melting and open-die forging works at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, forges 1.3932 into bar, rings, discs, sleeves and blanks to customer drawings and releases them with EN 10204 3.1 or 3.2 certification. Contact sales@steelforgepieces.com or +86 189 2135 9659.

---

## 1. What 1.3932 is, and what it is not

1.3932 is a precision alloy with special physical properties. It is not a structural steel and not a corrosion-resisting one. The material number says as much.

Under EN 10027-2 the digits after the decimal point put a material into a family. The range 1.36xx to 1.39xx is set aside for iron materials with special physical properties, meaning alloys bought for how they expand, conduct or behave in a magnetic field rather than for strength or corrosion resistance. 1.3932 falls in that range, next to its usual partner Invar 36 (1.3912) and the sealing alloys 1.3917 (Alloy 42) and 1.3927.

The chemistry is plain: about 20 % nickel, 6 to 7 % manganese, balance iron, with silicon and carbon held down as residuals. Nickel and manganese are both austenite stabilisers, so the structure is face-centred cubic at room temperature and stays that way. There is no hardening transformation to heat treat for. The composition is tuned for the expansion coefficient and, second to that, for electrical resistivity, since those two figures decide how a bimetal strip made from the alloy deflects and how much it self-heats when current passes through it.

### A correction to older listings

For several years this page, along with a number of other trader listings for 1.3932, described the grade as a stainless steel suitable for nitric acid coolers, seawater desalination, polythionic acid service and food processing. That text belonged to a different alloy. It has been removed.

1.3932 contains no chromium. There is no passive film, no pitting resistance and no corrosion resistance of any kind, and bare parts rust in humid air. If a drawing calls for 1.3932 in a wet or chemically aggressive duty, the drawing is most likely wrong and should be queried before material is bought.

What the alloy is good at is moving predictably when it gets hot. That property, used in a bonded strip, is the basis of a large family of thermal switches and controls.

---

## 2. Designations and equivalents

Drawings reach us under all of the names below. They describe the same nominal Fe-20Ni-6Mn chemistry. We accept orders under any of them and cross-list the equivalents on the material certificate.

| System or body | Designation | Notes |
|---|---|---|
| EN / DIN material number | 1.3932 | Werkstoffnummer. The safest single identifier for a purchase order |
| EN / DIN name | NiMn20-6 | Also written NiMn 20-6 and NiMn20/6 |
| SEW | SEW 385 | Eisenlegierungen mit besonderer Waermeausdehnung, iron alloys with special thermal expansion. The primary chemistry specification |
| DIN (bimetal) | DIN 1715-1 | Thermostat metals, technical delivery conditions. Covers the bonded composite rather than the single component |
| DIN (older) | DIN 17151 | Withdrawn, still quoted on legacy drawings |
| China | Ni20Mn6 | Standard Chinese precision-alloy designation |
| China (bimetal strip) | GB/T 4461 | Thermostatic bimetal strip. Ni20Mn6 is a listed active-layer component |
| ASTM | ASTM B753 | Standard Specification for Thermostat Component Alloys, the closest American framework |
| Shop names | Fe-20Ni-6Mn, FeNi20Mn6, 20Ni-6Mn | Informal but common on enquiries |

Standards are cited at the revisions known to us at the last page review. For procurement, reference the revision in force at the contract date.

**Naming trap: 1.3932 is not 1.3952.** The two numbers differ by one digit and get confused on enquiries regularly. 1.3952 is X2CrNiMoN18-14-3, a non-magnetic chromium-nickel-molybdenum austenitic stainless steel used where both corrosion resistance and low permeability are required. 1.3932 is a chromium-free Fe-Ni-Mn expansion alloy with no corrosion resistance at all. If your enquiry mentions corrosion, permeability limits or pressure-retaining service, the grade you want is probably 1.3952 or 1.3964.

---

## 3. Chemical composition of 1.3932 (NiMn20-6)

The table below is the SEW 385 baseline we work to. Nickel and manganese together set the expansion coefficient and hold the structure austenitic, and everything else is held low because residuals shift the expansion curve and interfere with roll bonding.

| Element | Min | Max | Metallurgical role |
|---|---|---|---|
| Nickel (Ni) | 19.0 | 21.0 | With Mn, stabilises austenite and sets the expansion coefficient and the Curie point. The controlled variable |
| Manganese (Mn) | 6.0 | 7.0 | Strong austenite stabiliser. Suppresses the Curie point below room temperature, which is what keeps expansion high |
| Silicon (Si) | - | 1.00 | Deoxidiser. Excess silicon embrittles and impairs bond quality |
| Carbon (C) | - | 0.20 | Kept low. Carbides distort the expansion curve and reduce formability |
| Iron (Fe) | Balance | | Matrix |
| P, S and residuals | - | low | Sulphur causes hot shortness during forging and delamination at the bond line |

Limits vary slightly between standard editions, mill practices and customer specifications. If your drawing imposes tighter limits, a narrower nickel band in particular, state them on the enquiry and we will confirm before accepting the order.

**Why the nickel band matters.** In the iron-nickel system the expansion coefficient changes steeply with nickel content around this composition. A drift of a few tenths of a percent moves the coefficient enough to measure, and with it the specific deflection of any bimetal made from the heat. If several parts of one assembly have to behave identically, specify single-heat supply on the purchase order.

**How we melt it.** We melt 1.3932 on site by electric arc furnace with ladle refining and vacuum oxygen decarburisation (EAF + LF + VOD), adding electroslag remelting where cleanliness or section size calls for it. Maximum heat size is 60 tonnes.

---

## 4. Physical properties

| Property | Typical value | Confidence |
|---|---|---|
| Mean CTE, 20 to 100 degC | about 20 x 10^-6 /degC | Design value, the property the alloy is bought for |
| Mean CTE, 20 to 200 degC | about 20 to 21 x 10^-6 /degC | Design value. The curve is close to linear across this band |
| Crystal structure | Austenitic, face-centred cubic | Established. Not hardenable by heat treatment |
| Magnetic behaviour | Paramagnetic at room temperature, Curie point below ambient | Established in principle. Specify a limit and we will measure it |
| Density | about 8.0 g/cm3 | Indicative. Use for forging-weight estimation only |
| Electrical resistivity | order of 1 microhm-m | Indicative and heat-dependent. Measured to ASTM B63 at 24 degC when required |
| Modulus of elasticity | about 150 to 180 GPa | Indicative |
| Corrosion resistance | None to speak of, no chromium | Established. Protect, plate or keep dry |

Expansion coefficient, structure and magnetic state are well established for this chemistry and can be used directly in design. The values marked indicative vary with heat, section size and condition, and are published for screening only. Where any physical value is contractually important, state it on the purchase order and we will report the measured result on the material certificate.

---

## 5. Thermal expansion and why the figure is high

The alloy is paramagnetic at room temperature, and that is what lets it expand freely.

In face-centred cubic iron-nickel alloys near 36 % nickel, a magnetostrictive volume contraction works against ordinary lattice expansion and cancels most of it. That is the Invar effect, and it is why Invar 36 barely moves when heated. The effect depends on the alloy being ferromagnetic. Above the Curie point it stops and expansion returns to normal.

1.3932 sits on the other side of that line by design. Nickel is dropped to about 20 % and 6 to 7 % manganese is added, which puts the Curie temperature below room temperature. In service the alloy is already paramagnetic, so nothing cancels the lattice expansion and it expands at the full rate of an austenitic metal, around 20 x 10^-6 /degC. That is roughly 1.7 times carbon steel and about fifteen times its Invar partner.

Mean coefficient of thermal expansion, 20 to 100 degC, in units of 10^-6 /degC:

| Alloy | CTE | Role |
|---|---|---|
| Invar 36 (1.3912) | 1.3 | Passive, low expansion |
| Alloy 42 (1.3917) | 5.3 | Sealing alloy |
| Carbon steel | about 12 | Reference |
| AISI 304 stainless | about 17 | Reference |
| **1.3932, NiMn20-6** | **about 20** | **Active, high expansion** |
| Mn75Ni15Cu10 | about 27 | Active, high expansion |

A thermostatic bimetal works on the difference between an active alloy and a passive one. Pairing 1.3932 with Invar 36 puts roughly 18 ppm/K of mismatch across the bond line, and that mismatch is the mechanism.

**Specify the temperature band.** Published coefficients are mean values between room temperature and a stated upper temperature, not instantaneous values at a point. A part cycling between 80 degC and 160 degC does not see the 20 to 100 degC figure. The coefficient also shifts with cold work and residual stress, which is why the alloy is used annealed.

---

## 6. How 1.3932 works inside a thermostatic bimetal

A thermostatic bimetal is two metal layers, sometimes three, bonded along their whole contact face. The layer with the larger expansion coefficient is the active component, and that is where 1.3932 goes. The layer with the smaller coefficient is the passive component, normally Invar 36 at 1.8 to 4.8 x 10^-6 /degC.

Heat the strip and the active side tries to grow while the passive side holds it back. The strip has nowhere to go but into an arc, curving towards the passive side. Cool it and the curvature reverses. Deflection at the free end is far larger than the length change of either layer on its own, and it repeats over millions of cycles.

Deflection rises with the expansion difference between the two layers and with the square of the free length, and falls with thickness. That is why strips are long and thin, and why the active alloy's coefficient is specified so tightly.

### Standard pairings and the third layer

A two-layer strip has whatever electrical resistance the two alloys happen to give it. Many applications heat the bimetal by passing current through it, and then the resistance has to match the current being switched. The usual answer is a third layer of nickel or copper between the active and passive layers, working as a shunt. Deflection stays about the same while resistivity drops by as much as an order of magnitude. Chinese grade 5J1411A, for example, is Ni20Mn6 active with a copper intermediate layer, to GB/T 4461.

| Layer | Purpose | Alloys commonly used |
|---|---|---|
| Active (high expansion) | Generates the motion. Marked on the convex side of the heated strip | Ni20Mn6 / NiMn20-6 (1.3932), Ni22Cr3, Mn75Ni15Cu10 |
| Passive (low expansion) | Restrains the active layer so the strip curves instead of stretching | Invar 36 (FeNi36, 1.3912), Ni42, Ni39 |
| Intermediate (shunt) | Sets the electrical resistivity and thermal conductivity without changing deflection much | Pure nickel, copper, plain steel |

**What we make and what we do not.** We are an open-die forging works. We supply 1.3932 in forged and machined form: bar, rings, discs, sleeves, blanks and tooling stock, melted here. We do not roll-bond or clad thermostatic bimetal strip and we do not stamp bimetal elements. Finished strip to DIN 1715 or GB/T 4461 needs a strip mill.

---

## 7. Mechanical properties

1.3932 is not a strength alloy. It is austenitic, cannot be hardened by heat treatment, and in service carries very little load, since a bimetal element develops force through thermal mismatch rather than through applied stress.

Typical values, annealed forged bar. Indicative, not specification minima.

| Property | Typical | Comment |
|---|---|---|
| Tensile strength Rm | 450 to 600 MPa | Mild-steel class. Rises substantially with cold work |
| Yield strength Rp0.2 | 180 to 280 MPa | Size the section for load, do not select this alloy for strength |
| Elongation A | 35 to 50 % | Ductile and readily formed in the annealed condition |
| Hardness, annealed | 130 to 170 HV | Cold-rolled strip runs far harder |
| Work hardening | Pronounced | Typical austenitic behaviour |

Cold work raises strength and ruins the expansion accuracy. Strain from drawing, straightening or heavy machining shifts the measured coefficient away from the datasheet value, then relaxes in service and moves the part. Where the expansion figure is the reason the alloy was chosen, the sequence is forge, anneal, rough machine, stress relieve, finish machine.

---

## 8. Forged forms and sizes we supply in 1.3932

Everything below is made to order against a drawing or a dimension list. There is no stock catalogue. Most commercial use of this alloy is as thin strip for bonding, so the forged forms here cover blank supply, research quantities, machined components and tooling.

| Form | Indicative range | Route and typical use |
|---|---|---|
| Forged round bar | 25 to 400 mm dia. | Cogged and turned. Machining stock, rolling-blank feedstock, test material |
| Forged flat bar and blocks | to 2,000 mm long | Pressed and cut. Blanks for slitting and laboratory work |
| Seamless rolled rings | OD 200 to 1,500 mm | Pierced and ring-rolled, continuous circumferential grain flow |
| Forged rings and sleeves | OD 80 to 1,000 mm | Upset and punched, or bored from solid |
| Discs and blanks | 100 to 1,200 mm dia. | Upset discs with radial grain flow. Rolling and stamping blanks |
| Hollow bar and bushings | OD 80 to 600 mm | Trepanned or forged over a mandrel |
| Near-net and special shapes | to drawing | Thermal-actuator bodies, spacers, instrument components |

Ranges describe routine work rather than hard limits. The works runs 6,300 t, 4,000 t and 2,000 t presses, 6 m, 3 m and 1 m radial-axial ring mills and a 60 t maximum heat.

Supply conditions: as-forged with machining allowance, rough machined, or finish machined to drawing. Annealed as standard. Minimum order is 10 kg, with no minimum piece count.

---

## 9. Forging, heat treatment, machining and welding

### Forging

1.3932 is hot worked from approximately 1,100 to 1,180 degC, finishing above roughly 900 degC. It is single phase austenitic, so there is no transformation to work around, but two cautions apply.

- Heat quickly and do not soak. Long residence in a sulphur-bearing furnace atmosphere lets sulphur into the surface and causes hot shortness and surface checking. Furnaces are run clean and neutral to slightly reducing.
- Stay away from the solidus. Overheating coarsens the grain irreversibly, and a coarse-grained precision alloy will not give consistent properties down the bar.

A forging reduction of at least 4:1 from the ingot breaks down the as-cast structure. After the final blow the piece is slow cooled and annealed. The anneal, not the forging, sets the expansion coefficient the customer will measure.

### Heat treatment

| Operation | Temperature | Time and cooling | Purpose |
|---|---|---|---|
| Full anneal | 850 to 1,000 degC | About 30 min per 25 mm section, protective atmosphere or vacuum, air or water cool | Removes cold work, restores the datasheet expansion coefficient, softens for machining |
| Stress relief / stabilise | 300 to 350 degC | 1 to 4 h, slow cool | Applied after final machining on precision parts, to lock dimensions before service |

The alloy scales readily and has no chromium to protect it, so where surface condition matters the anneal is run under a protective atmosphere.

### Machining

Machining behaves like austenitic stainless steel. The alloy is gummy, work hardens under a rubbing tool and throws long stringy chips. Use sharp positive-rake carbide tooling replaced at the first sign of edge rounding, short rigid setups, flood coolant, heavy positive feeds, and no dwelling in the cut. Leave 2 to 4 mm of stock after roughing, stress relieve, then finish with light depths of cut.

### Welding and joining

1.3932 welds by GTAW, electron beam and resistance methods with a matching Fe-Ni-Mn filler. Joint faces have to be clean, since sulphur and low melting point contamination cause cracking. Where the joint has to share the parent metal's expansion behaviour, a post-weld anneal is needed. In its intended use the alloy is not welded at all but roll bonded, which is a solid state cold pressure weld carried out at the strip mill.

---

## 10. Where 1.3932 is used

| Sector | Typical components | Why this alloy |
|---|---|---|
| Low-voltage switchgear | Miniature circuit breakers, motor protectors, overload releases, thermal cut-outs | Heated directly by the load current, trips on a defined temperature rise. The highest-volume use |
| Domestic appliances | Iron and kettle regulators, oven and cooker thermostats, refrigerator and freezer controls, snap discs | Cheap, sturdy, self-contained control needing no electronics or power |
| Automotive and e-mobility | Seat-heater controls, cooling-water and exhaust thermostats, flashers, battery-pack thermal cut-outs | Survives vibration and wide temperature swings, fails safe |
| Measurement and instruments | Bimetal dial thermometers, exhaust gas thermometers, spiral and helical measuring coils, temperature compensation elements | Linear deflection over a wide band with no power supply |
| Energy and environmental plant | Time-delay switches, regulators, starters, thermal relays, over-temperature protection | Long-life repeatable actuation, millions of cycles |
| Lighting | Fluorescent and energy-saving lamp starters, flasher units | Very thin strip, fast thermal response |

In forged form specifically, 1.3932 goes into rolling and stamping blanks for the strip mills that make the above, into machined bodies and spacers for thermal actuators, and into research and qualification quantities.

---

## 11. Limitations to design around

| Limitation | Consequence | Practical response |
|---|---|---|
| No corrosion resistance | Rusts in damp air like plain carbon steel | Plate, paint, oil or keep dry. Never specify it for wet or chemical duty |
| Low strength | Yield around 200 MPa, mild-steel class | Size the section for load, or select a different alloy |
| Expansion is process-sensitive | Cold work, residual stress and heat treatment all shift the coefficient | Specify the coefficient and temperature band on the drawing |
| Heat-to-heat variation | A few tenths of a percent of nickel moves the coefficient enough to measure | Specify single-heat supply where parts must behave identically |
| Oxidation and scaling | Scales readily at annealing temperature | Protective-atmosphere or vacuum anneal where surface condition matters |
| Machining behaviour | Gummy, work hardening, stringy chips, short tool life | Sharp tools, flood coolant, no dwell, stress relief between roughing and finishing |
| Not a structural or pressure grade | Not listed in pressure-vessel or piping codes | If the part is pressure retaining, this is the wrong alloy |

---

## 12. 1.3932 compared with neighbouring grades

| Grade | Nominal composition | CTE (10^-6 /degC) | Choose it when |
|---|---|---|---|
| 1.3932, NiMn20-6 | Fe-20Ni-6Mn | about 20 | You need the high-expansion half of a bimetal pair |
| Ni22Cr3 | Fe-22Ni-3Cr | about 19 to 20 | Similar deflection with some oxidation resistance from the chromium |
| Mn75Ni15Cu10 | Mn-Ni-Cu | about 27 | Maximum deflection wanted, service temperature modest |
| Invar 36, 1.3912 | Fe-36Ni | about 1.3 | The passive layer, or any part that must not change length |
| Alloy 42, 1.3917 | Fe-42Ni | about 5.3 | Matching silicon, alumina or a hard sealing glass |
| Alloy 48 / Alloy 52 | Fe-48Ni / Fe-51Ni | 8.7 / 10.0 | Sealing to soft and soda-lime glass |
| 1.3952, X2CrNiMoN18-14-3 | Fe-18Cr-14Ni-3Mo-N | about 16 | You actually wanted a non-magnetic stainless steel |
| Nitronic 50, 1.3964 | Fe-22Cr-12Ni-2Mo-N | about 16 | Non-magnetic, high strength and corrosion resistant |

We forge all of the grades above. If you are still choosing, send the operating temperature range, the movement or tolerance you need to hold and the environment.

---

## 13. Testing, inspection and certification

Because the steel is melted here, chemistry is verified at the furnace rather than taken from a supplier certificate.

| Test | Standard | Included |
|---|---|---|
| Chemical analysis, ladle and product | SEW 385, ASTM E415 (OES) | Standard |
| Tensile test | ASTM A370, EN ISO 6892-1 | Standard |
| Hardness | ASTM E10 / E140, EN ISO 6506 | Standard |
| Ultrasonic examination | EN 10228-3, SEP 1921, ASTM A388 | Standard, acceptance class to order |
| Dimensional report and heat-treatment chart | To drawing, furnace record | Standard |
| Thermal expansion by dilatometry | ASTM E228, ASTM E831 | On request. Recommended |
| Electrical resistivity | ASTM B63, at 24 degC | On request |
| Magnetic permeability | To agreed method and limit | On request |
| Grain size and micrograph | ASTM E112 | On request |
| PMI verification | XRF / OES | On request |

Forgings are released with an EN 10204 3.1 certificate issued against the mill heat, or EN 10204 3.2 witnessed by a third party such as TUV, SGS, BV, Lloyd's Register or DNV when the order calls for it. The works holds CCS, BV, DNV, LR and NK classification society approvals.

---

## 14. How to specify a 1.3932 order

The expansion requirement has to be stated explicitly, because it is the property being bought and the chemistry alone does not guarantee it. Send a drawing to sales@steelforgepieces.com with the items below and a quotation normally comes back within two working days.

1. Grade and standard: "1.3932 / NiMn20-6 to SEW 385", or the designation your drawing uses.
2. Drawing or dimensions: PDF, DWG, DXF or STEP, or simply OD x ID x length.
3. Product form: bar, ring, disc, sleeve, blank or machined part.
4. Expansion requirement: the value, the temperature band, and whether it must be measured and certified.
5. Single-heat requirement: state it if several pieces must behave identically.
6. Supply condition: as-forged, rough machined or finish machined. Annealed as standard.
7. Test and certification scope: EN 10204 3.1 or 3.2, UT class, any additional tests.
8. Quantity, delivery terms, destination port and required date.

Copy-ready drawing callout:

```
MATERIAL       1.3932 / NiMn20-6 to SEW 385 (Ni20Mn6, GB/T 4461)
CONDITION      Annealed, protective atmosphere.
               Stabilise 320 degC / 2 h after final machining
EXPANSION      Mean CTE 20 x 10^-6 /degC over 20-100 degC, tolerance to be agreed.
               Measured on the delivered heat by dilatometry, reported on the MTC
HEAT CONTROL   All pieces of this assembly from a SINGLE HEAT
NDE            UT per EN 10228-3, quality class to order
CERTIFICATION  EN 10204 3.1 mill certificate (3.2 with third-party witness where stated)
SURFACE        Oiled and VCI wrapped for shipment. No chromium, protect from moisture
MARKING        Heat number, grade and drawing number, on a non-functional surface
```

Minimum order is 10 kg with no minimum piece count. Normal lead time runs 20 to 60 days from order confirmation.

---

## 15. Frequently asked questions

**What is material 1.3932?**
1.3932 is the EN and DIN material number for NiMn20-6, an austenitic iron-nickel-manganese alloy containing 19.0 to 21.0 % nickel, 6.0 to 7.0 % manganese, up to 1.0 % silicon and up to 0.20 % carbon with the balance iron, specified by SEW 385 and designated Ni20Mn6 in China. It belongs to the EN 10027-2 group of iron materials with special physical properties, and it is bought for a high coefficient of thermal expansion of about 20 x 10^-6 /degC, which makes it the standard high-expansion active layer of thermostatic bimetals. Jiangyin Jiangnan Metal Co., Ltd., an open-die forging works in Jiangyin, Jiangsu, China, melts and forges 1.3932 into bar, rings, discs and blanks to customer drawings.

**Is 1.3932 a stainless steel?**
No. 1.3932 contains no deliberate chromium and has no corrosion resistance, so bare parts rust in damp air much like plain carbon steel. It is a precision expansion alloy rather than a corrosion-resisting one. Some supplier listings, including an earlier version of this page, filed 1.3932 under stainless steel and described nitric acid, seawater and food-processing service. That text came from a different alloy and is incorrect. If your application needs both non-magnetic behaviour and corrosion resistance, the grade you want is probably 1.3952 (X2CrNiMoN18-14-3) or 1.3964.

**What is the coefficient of thermal expansion of NiMn20-6?**
The mean coefficient of thermal expansion of 1.3932 / NiMn20-6 is approximately 20 x 10^-6 /degC measured from 20 degC to 100 degC, and stays close to that value through about 200 degC. For comparison, plain carbon steel is near 12, AISI 304 stainless near 17, and the Invar 36 the alloy is normally bonded to is near 1.3. That difference of roughly 18 ppm/K across the bond line is what makes a thermostatic bimetal bend.

**Is 1.3932 magnetic?**
1.3932 is austenitic with a Curie point below room temperature, so it is effectively non-magnetic, that is paramagnetic, at ambient temperature. This is not incidental. It is the reason the alloy expands so much. In iron-nickel alloys near 36 % nickel a magnetostrictive contraction cancels most of the lattice expansion, producing the Invar effect. Lowering nickel to 20 % and adding 6 to 7 % manganese pushes the Curie point below ambient, the cancelling contribution never operates, and the alloy expands at the full austenitic rate.

**What is 1.3932 used for?**
1.3932 is used almost exclusively as the active, high-expansion component of thermostatic bimetal. Bonded to a low-expansion passive layer such as Invar 36, it makes strips, discs and coils that bend by a known amount as temperature changes. Those elements sit inside miniature circuit breakers, motor overload protectors and thermal cut-outs; in thermostats for irons, kettles, ovens, refrigerators and cooking appliances; in automotive cooling-water, exhaust and seat-heater controls; in bimetal dial and exhaust gas thermometers; and in fluorescent lamp starters, flashers and time-delay switches.

**What standards cover 1.3932 / NiMn20-6?**
The chemistry is specified by SEW 385, the Stahl-Eisen-Werkstoffblatt for iron alloys with special thermal expansion. The bonded thermostatic bimetal composite that uses it is covered by DIN 1715-1 in Germany and by GB/T 4461 in China, where the alloy is designated Ni20Mn6. ASTM B753 is the closest American framework for thermostat component alloys. The older DIN 17151 is sometimes quoted on legacy drawings.

**Can 1.3932 be forged, and at what temperature?**
Yes. 1.3932 is hot worked from approximately 1,100 to 1,180 degC with the finishing temperature held above roughly 900 degC. The alloy is single phase austenitic, so there is no transformation to work around, but it should be heated quickly rather than soaked. Prolonged residence in a sulphur-bearing furnace atmosphere causes hot shortness and surface checking, and overheating near the solidus coarsens the grain irreversibly. The subsequent full anneal at about 850 to 1,000 degC, rather than the forging itself, is what sets the expansion coefficient the customer will measure.

**What is the difference between 1.3932 and 1.3952?**
They are entirely different materials that differ by one digit in the material number. 1.3932 (NiMn20-6) is a chromium-free iron-nickel-manganese expansion alloy, bought for a high coefficient of thermal expansion near 20 ppm/K, with no corrosion resistance and no structural role. 1.3952 (X2CrNiMoN18-14-3) is a non-magnetic chromium-nickel-molybdenum austenitic stainless steel with high corrosion resistance and low magnetic permeability. If your requirement mentions corrosion, chlorides, permeability limits or pressure-retaining duty, you almost certainly want 1.3952.

**Do you supply finished thermostatic bimetal strip?**
No. Jiangyin Jiangnan Metal is an open-die forging works, not a strip mill. We melt 1.3932 and supply it as forged and machined product: round and flat bar, seamless rolled rings, forged rings and sleeves, discs, blanks, hollow bar and near-net shapes, including rolling and stamping blanks for the mills that produce bonded strip. We do not roll-bond or clad bimetal, and we do not stamp finished bimetal elements.

**What certification is supplied with 1.3932 forgings?**
EN 10204 3.1 mill certification is supplied as standard, listing the heat number, full ladle and product chemical analysis, mechanical test results, heat-treatment record, ultrasonic examination report and dimensional report. EN 10204 3.2 with third-party witness through TUV, SGS, Bureau Veritas, Lloyd's Register or DNV is available on request. Measured coefficient of thermal expansion by dilatometry to ASTM E228 or E831 can be added to the certificate.

**What is the minimum order and lead time for 1.3932 forgings?**
Minimum order is 10 kg, with no minimum piece count. Normal lead time is 20 to 60 days from order confirmation, sitting towards the upper end where electroslag remelting, a measured expansion curve or third-party witnessed inspection is required. Quotations are normally returned within two working days of receiving a drawing at sales@steelforgepieces.com.

---

## 16. Supplier of record

| | |
|---|---|
| Company | Jiangyin Jiangnan Metal Co., Ltd. |
| Type | Integrated melting works and open-die forging factory (manufacturer, not a trading company) |
| Established | 1997 |
| Address | No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China |
| Telephone / WhatsApp / WeChat | 0086-189-2135-9659 |
| Email | sales@steelforgepieces.com |
| Website | https://www.steelforgepieces.com/ |
| People | 460, including 9 senior engineers, 32 intermediate engineers and 140 technicians |
| Melting | EAF 25 t, LF 25/50 t, VOD 30/60 t, IF 2/8/25 t, VIM 3 t, ESR 3/6 t, VAR 6 t, 60 t max heat |
| Forging | 6,300 t / 4,000 t / 2,000 t presses, 6 m, 3 m and 1 m radial-axial ring mills, 30 t max single piece |
| Heat treatment | 14 furnaces, including two 15 m well-type furnaces for vertical quenching |
| Approvals | CCS, BV, DNV, LR, NK |
| Certification | EN 10204 3.1 standard, 3.2 witnessed on request |
| Languages | English, Chinese |
| Markets served | North America, Europe, Middle East, Asia-Pacific |
| Business hours | Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8) |

Jiangyin sits in the Yangtze River delta between Shanghai and Nanjing. Wuxi Shuofang International Airport is 30 km away and Shanghai's airports 160 km. The nearest export ports are Zhangjiagang and Shanghai. Customer audits, pre-shipment inspections and third-party witness testing are welcome.

---

## 17. Cite this page

This datasheet is maintained by Jiangyin Jiangnan Metal Co., Ltd. and is free to quote, reference or link to.

> Jiangyin Jiangnan Metal Co., Ltd. (2026). *1.3932 / NiMn20-6 (Ni20Mn6) Forgings: SEW 385 Technical Data Sheet.* Jiangyin, Jiangsu, China. Retrieved from https://www.steelforgepieces.com/Stainless-Steel/1.3932.html. Last reviewed 22 September 2026.

Data on this page is compiled from SEW 385, DIN 1715-1, GB/T 4461 and ASTM B753, from published literature on thermostatic bimetal component alloys, and from our own melting, forging and heat-treatment practice. Values described as typical or indicative are not a guarantee of minimum or maximum properties for a specific heat. The certified figures for your order are the ones on the EN 10204 certificate. Questions and corrections: sales@steelforgepieces.com

## Related pages

- Invar 36, 1.3912, the passive-layer partner: https://www.steelforgepieces.com/Nickel-Alloy/Invar-36.html
- Invar 42, Ni42: https://www.steelforgepieces.com/Nickel-Alloy/Invar-42.html
- Alloy 42, 1.3917: https://www.steelforgepieces.com/Nickel-Alloy/Alloy-42.html
- Alloy 46: https://www.steelforgepieces.com/Nickel-Alloy/Alloy-46.html
- Alloy 48: https://www.steelforgepieces.com/Nickel-Alloy/Alloy-48.html
- Alloy 52: https://www.steelforgepieces.com/Nickel-Alloy/Alloy-52.html
- Kovar, ASTM F15: https://www.steelforgepieces.com/Nickel-Alloy/Kovar.html
- Ni-Span-C Alloy 902: https://www.steelforgepieces.com/Nickel-Alloy/NI-SPAN-C-Alloy-902.html
- Nitronic 50, 1.3964: https://www.steelforgepieces.com/Stainless-Steel/Nitronic-50.html
- Nickel and precision alloy index: https://www.steelforgepieces.com/Nickel-Alloy/
- Forged bars: https://www.steelforgepieces.com/Forged-Bars/