Seamless rolled rings
Ring-rolled from a punched preform on the radial-axial mills, rectangular or contoured section, to OD 6,000 mm.
Home / Stainless Steel / UNS S31009
Heat-resisting austenitic stainless steel · 25Cr-20Ni
UNS S31009 is the high-carbon modification of Alloy 310, developed for enhanced creep resistance at elevated temperature. Carbon is controlled to a 0.04 to 0.10 percent band, a specified minimum as well as a maximum, and ASTM A182 calls for a coarse grain size of No. 6 or coarser. The low-carbon counterpart is 310S, UNS S31008, used where fabrication matters more than creep strength.
This works melts its own steel and forges it on the same site, so a finished S31009 part traces back to its melt number rather than to a purchased billet. Orders start at 10 kg with no minimum piece count.
All three grades share the same 25Cr-20Ni base. Carbon and silicon separate them, and carbon decides whether a part holds its shape under sustained load at temperature.
| Grade | UNS | Carbon | Silicon | Reason for selection |
|---|---|---|---|---|
| 310 | S31000 | 0.25 | 1.50 | General high-temperature corrosion resistance |
| 310S | S31008 | 0.08 | 1.50 | Low-carbon version, used for ease of fabrication and better weldability |
| 310H | S31009 | 0.04 to 0.10 | 0.75 | High-carbon modification for enhanced creep resistance |
Because the carbon ranges overlap, the grain size and carbon content of a given lot can often satisfy both the 310S and the 310H requirements at once, which is why dual-certified 310S/310H material is common on the market. Dual certification is a property of the actual heat and not a general equivalence. Where creep strength governs the design, order S31009 by name and call for the grain size and carbon results on the certificate.
| Element | ASTM A182 F310H, forgings | 310H per A240 and published data sheets |
|---|---|---|
| Carbon, C | 0.04 to 0.10 | 0.040 to 0.10 |
| Chromium, Cr | 24.0 to 26.0 | 24 to 26 |
| Nickel, Ni | 19.0 to 22.0 | 19 to 22 |
| Manganese, Mn | 2.00 max | 2.00 max |
| Silicon, Si | 1.00 max | 0.75 max |
| Phosphorus, P | 0.045 max | 0.045 max |
| Sulfur, S | 0.030 max | 0.030 max |
| Iron, Fe | Balance | Balance, about 45.9 to 49.1 |
The 0.75 percent silicon figure in general circulation comes from plate data sheets. For forgings ordered to A182 F310H the limit is 1.00 percent maximum. State which limit your specification imposes at enquiry stage, since it affects heat selection.
Clause 8.2 of A182 prohibits grades to which lead, selenium or other elements have been added to render the material free-machining. Clause 8.3 prohibits starting material produced to a specification that requires any element beyond those listed for the grade. Material is purchased and melted on that basis.
The A182 minima are the acceptance criteria. Published typical values vary between sources and are listed separately for orientation only.
| Property | Metric | Inch-pound |
|---|---|---|
| Tensile strength, min | 515 MPa | 75 ksi |
| Yield strength, min | 205 MPa | 30 ksi |
| Elongation in 50 mm or 4D, min | 30 % | 30 % |
| Reduction of area, min | 50 % | 50 % |
| Brinell hardness | Not specified by A182 for this grade | |
| Property | Sandmeyer Steel, typical at 20 C | AZoM, annealed 310H |
|---|---|---|
| Tensile strength | 550 MPa / 80 000 psi | 515 MPa / 74 700 psi |
| Yield strength, 0.2 % offset | 245 MPa / 35 000 psi | 205 MPa / 29 700 psi |
| Elongation | 45 % min in 2 in. | 40 % in 50 mm |
| Hardness | 217 Brinell max | 217 Brinell / 95 HRB |
| Modulus of elasticity | 196 GPa / 28.5 x 106 psi | 200 GPa / 29 000 ksi |
| Shear modulus | Not stated | 77.0 GPa / 11 200 ksi |
| Poisson's ratio | Not stated | 0.3 |
One tension test is made for each heat of austenitic grades. Specimens are not removed until all heat treatment is complete, and for austenitic and ferritic-austenitic grades the specimen may be taken from any convenient location. Where test blanks are used they receive approximately the same working as the finished product, are heat treated with it, and approximate its maximum cross section.
| Property | Value |
|---|---|
| Density | 7.89 g/cm3 / 0.285 lb/in3 |
| Melting range | 1354 to 1402 C / 2470 to 2555 F |
| Specific heat, 0 to 100 C | 502 J/kg·K / 0.12 BTU/lb·F |
| Thermal conductivity at 100 C | 10.8 W/m·K / 8.0 BTU/hr/ft2/ft/F |
| Electrical resistivity at 20 C | 78.0 microhm·cm |
| Modulus of elasticity | 196 GPa / 28.5 x 106 psi |
Creep performance is the reason the H grade exists. Typical published values for Alloy 310, in MPa.
| Temperature | Creep strain | Creep rupture | ||||
|---|---|---|---|---|---|---|
| 1 000 h | 10 000 h | 100 000 h | 1 000 h | 10 000 h | 100 000 h | |
| 600 C / 1112 F | 120 | 100 | 40 | 200 | 140 | 80 |
| 700 C / 1292 F | 50 | 35 | 20 | 80 | 45 | 20 |
| 800 C / 1472 F | 20 | 10 | 8 | 35 | 20 | 8 |
| 900 C / 1652 F | 10 | 6 | 3 | 15 | 10 | 5 |
| 1000 C / 1832 F | 5 | 3 | 1.5 | 9 | 4 | 2 |
These figures suit preliminary sizing. Code-qualified allowable stresses for S31009 must be taken from ASME Boiler and Pressure Vessel Code Section II, Part D at the design temperature.
Published limits differ because sources assume different atmospheres and different definitions of continuous service. Both commonly cited sets are reproduced rather than averaged.
| Condition | Limit | Source |
|---|---|---|
| Oxidation resistance, mildly cyclic conditions | 1100 C / 2010 F | Sandmeyer Steel |
| Oxidizing, sulfur up to 2 g/m3, continuous | 1050 C / 1922 F | Sandmeyer Steel |
| Oxidizing, sulfur up to 2 g/m3, peak | 1100 C / 2012 F | Sandmeyer Steel |
| Oxidizing, sulfur above 2 g/m3 | 950 C / 1742 F | Sandmeyer Steel |
| Low oxygen atmosphere, sulfur up to 2 g/m3 | 1000 C / 1832 F | Sandmeyer Steel |
| Nitriding or carburizing atmosphere | 850 to 950 C / 1562 to 1742 F | Sandmeyer Steel |
| 310H, intermittent service | 1040 C / 1904 F | AZoM |
| 310H, continuous service | 1150 C / 2102 F | AZoM |
| Cryogenic use, low magnetic permeability and toughness | down to -268 C / -450 F | Sandmeyer Steel |
AZoM advises against continuous service between 425 and 860 C, 797 to 1580 F, because of carbide precipitation. Separately, Alloy 310 is subject to sigma phase precipitation when held between 650 and 950 C, 1202 to 1742 F, and a solution annealing treatment at 1100 to 1150 C, 2012 to 2102 F, will restore a degree of toughness. Frequent thermal cycling also reduces oxidation resistance.
Alloy 310 is not designed for service in wet corrosive environments. The high carbon content present to enhance creep properties has a detrimental effect on aqueous corrosion resistance, and the alloy is prone to intergranular corrosion after long-term exposure at high temperature. Set against that, its 25 percent chromium content makes it more corrosion resistant than most heat-resisting alloys.
At temperature the high chromium and silicon content give resistance to sulfidation, and the alloy can be used in moderately carburizing atmospheres. More severe carburizing atmospheres in thermal process equipment usually call for a nickel alloy such as Alloy 330, UNS N08330. In reducing, nitriding or carburizing atmospheres 310H does not perform as well as Alloy 600, UNS N06600 or Alloy 800, UNS N08800, though it does outperform most heat-resisting stainless steels in those conditions.
Where the duty is wet and aggressive rather than hot, 904L, Sanicro 28 or Hastelloy C-276 are the more suitable forging grades.
Clause 6.2 of A182 requires stainless steels to be melted by electric furnace, with the option of separate degassing and refining, by vacuum furnace, or by either of those followed by vacuum or electroslag consumable remelting. Clause 6.3 requires sufficient discard to secure freedom from injurious piping and undue segregation.
This plant covers those routes in house. S31009 runs through the 25 t electric arc furnace, is refined in a 25 t or 50 t ladle furnace and decarburised under vacuum in the 30 t or 60 t VOD units where low carbon or tight nitrogen control is wanted. Maximum heat size is 60 tonnes. Protective-atmosphere electroslag remelting at 3 t and 6 t, and vacuum arc remelting at 6 t, are available where a specification or a heavy section calls for a remelted ingot.
Material is forged as close as practicable to the specified shape and size, with uniform heating at 950 to 1200 C. Two restrictions in A182 bear directly on how S31009 piping components may be made. Clause 6.4.1 states that flanges of any type, elbows, return bends, tees and header tees shall not be machined directly from bar stock. Clause 6.4.2 permits cylindrically shaped parts to be machined from forged or rolled solution-annealed austenitic stainless steel bar without additional hot working. A quotation for bar-machined 310H flanges does not meet the specification.
Clause 1.2 limits products made to A182 to a maximum weight of 10 000 lb, 4540 kg, and refers larger austenitic products to A965/A965M. Both specifications are quoted here.
| Requirement | Value | Clause |
|---|---|---|
| Heat treat type | Solution treat and quench | A182 Table 1 |
| Solutioning temperature, minimum | 1900 F [1040 C] | A182 Table 1 |
| Cooling media | Liquid | A182 Table 1 |
| Quenching, cool below | 500 F [260 C] | A182 Table 1 |
| Cooling after hot working, before heat treating | Below 1000 F [538 C] | A182 7.1 |
| Direct quench from hot-working heat | Not permitted for F310H | A182 7.3.1 |
| Grain size | ASTM No. 6 or coarser, per E112 | A182 10.1.1 |
Clause 7.3.1 allows many austenitic grades to be individually rapidly quenched immediately after hot working while still above the minimum solution annealing temperature. F310H is named in the list of grades excluded from that option, together with F304H, F309H, F310, F316H, F321, F321H, F347, F347H, F348, F348H, F45 and F56. Every S31009 forging therefore receives a separate solution anneal and liquid quench with a recorded furnace chart.
Solution annealing above the 1040 C minimum is carried out in the three high-temperature car-bottom furnaces on site, working chamber 3,500 x 1,300 x 1,100 mm. Long shafts are quenched vertically in the two 15 m well-type furnaces. After hot forming, a final anneal at 1000 to 1150 C followed by rapid quenching is the recommended practice for this alloy family. Heat treatment of forgings may be performed before machining.
The alloy is quite ductile and cold forms in a manner very similar to 316. Cold forming of pieces that will see long-term exposure to high temperature is not recommended, since the alloy is subject to carbide precipitation and sigma phase precipitates.
Alloy 310 can be readily welded by most standard processes, including TIG, plasma, MIG, SMAW, SAW and FCAW. Where the best corrosion resistance after welding is required, the low-carbon 310S variant is preferred to minimise carbide precipitation, which is a further reason to settle early whether the application is creep driven or fabrication driven.
Ultrasonic examination follows EN 10228-4, the part of the standard covering ultrasonic testing of austenitic and austenitic-ferritic stainless steel forgings. EN 10228-3 applies to ferritic and martensitic forgings and is not the correct part for this grade. ASTM A388/A388M, referenced by A182, is available as an alternative acceptance basis, as is SEP 1921 where a customer specification calls for it.
On-site testing covers optical emission spectrometry to ASTM E415, infrared carbon and sulphur analysis to ASTM E1019, handheld positive material identification, tensile testing on 600 kN and 300 kN machines to ASTM A370, Charpy V-notch impact to minus 60 C, ultrasonic flaw detection, and metallographic grain size measurement to ASTM E112, which is the method the A182 grain size requirement calls for.
Intergranular corrosion testing to ASTM A262 or ASTM G28 is placed with an accredited third-party laboratory and the report is issued alongside the mill certificate. Other supplementary requirements of A182 can be added to the order, among them liquid penetrant examination to E165 and macroetch testing to E340. Magnetic particle examination is not applicable to this grade, which is non-magnetic in the solution annealed condition.
Inspection documents are issued to EN 10204 Type 3.1, validated by an inspection representative independent of the manufacturing department and reporting results on the specific heat, or to Type 3.2, witnessed by BV, DNV, LR, SGS, TUV or the customer's own inspector. Nominate the inspection body on the purchase order. The works holds CCS, BV, DNV, LR and NK approvals.
Ring-rolled from a punched preform on the radial-axial mills, rectangular or contoured section, to OD 6,000 mm.
Upset and punched rings for sections outside the ring-mill envelope, retaining rings and valve seat rings.
Weld neck, blind, slip-on, socket weld, lap joint, orifice and long weld neck to ASME B16.5 and B16.47, or to drawing.
Stepped, eccentric and crankshaft forgings, furnace fan and roller shafts, to 14,000 mm turned length.
Solid forged discs, tube sheets and covers, supplied proof-machined for volumetric inspection.
Bored hollow sections, liners and couplings, bored from solid forged blanks.
Forged round, flat and square bar and blocks, the feedstock route for machined bodies and tooling.
Valve bodies, bonnets, stems, seat rings, blocks, nozzles and manifolds, with heavy-wall pipe sections.
Melting, forging, ring rolling, heat treatment, machining and inspection are all on one site. No forging, heat treatment or machining step is subcontracted.
| Product | Limit | Set by |
|---|---|---|
| Seamless rolled rings | up to OD 6,000 mm | 6 m radial-axial ring mill, with 3 m and 1 m mills for smaller sizes |
| Minimum ring size | from OD 50 mm | Upset-and-punch route below ring-mill range |
| Forged shafts | up to 14,000 mm turned length | C61160 horizontal lathe, 15 m well furnace for vertical quench |
| Discs, tube sheets, blocks | up to 5,000 mm machined diameter | 5,000 mm vertical turning lathe |
| Bored cylinders and hollow shafts | up to 1,600 mm dia x 10,000 mm | CNC deep-hole drilling machine |
| Single-piece weight | up to 30,000 kg | 60 t heat size, 6,300 t press |
| Minimum order | 10 kg, no minimum piece count | Works policy |
| Lead time | 20 to 60 days | Works policy |
Presses are 6,300 t, 4,000 t and 2,000 t, with hammers at 5 t, 3 t, 2 t, 1 t and 750 kg for drawing out and small batch work. Heat treatment runs across 14 furnaces, including three high-temperature car-bottom furnaces and two well-type furnaces 15,000 mm deep by 1,500 mm diameter.
| Sector | Components |
|---|---|
| Furnaces | Burners, doors, fans, piping, recuperators |
| Fluidized bed furnaces | Coal combustors, grids, piping, wind boxes |
| Ore processing and steel plants | Smelter and steel melting equipment, continuous casting equipment |
| Petroleum refining | Catalytic recovery systems, flares, recuperators, tube hangers |
| Power generation | Coal gasifier internals, pulverized coal burners, tube hangers |
| Sintering and cement plants | Burners, burner shields, feeding and discharging systems, wind boxes |
| Thermal processing | Annealing covers and boxes, burner grids, doors, fans, muffles and retorts, recuperators, walking beams |
| Food processing | Equipment handling hot organic acids |
| Cryogenic | Cryogenic components and structures |
| System | Designation | Note |
|---|---|---|
| UNS | S31009 | Exact |
| AISI and common usage | 310H | Exact |
| ASTM and ASME, forgings | A182/A182M F310H, SA-182 F310H, A965/A965M | Governing specifications for forged parts |
| ASTM, plate | A240 310H, SA240, AMS 5521 | Plate product forms |
| Werkstoff number | 1.4845 | Listed for the 310 / 310S / 310H family, corresponds most closely to 310S, not an exact S31009 equivalent |
| JIS | SUS310S | Equivalent to the low-carbon grade, approximate only |
| Related grades | S31000, S31008, N08330 | Select by carbon level and atmosphere |
Other heat-resisting and high-temperature forging grades produced here: 347H, F321 and 321H, F347, 330, A286, Incoloy 800H, 800HT, Inconel 617, Haynes 230 and Hastelloy X.
High carbon. S31009, designated 310H, is the high-carbon modification developed for enhanced creep resistance, with carbon between 0.04 and 0.10 percent. The low-carbon version is 310S, S31008, at 0.08 percent maximum, used for ease of fabrication. Plain 310, S31000, permits up to 0.25 percent carbon.
Solution treat and quench. Table 1 of A182 gives a minimum solutioning temperature of 1900 F [1040 C], liquid cooling media, and quenching to below 500 F [260 C]. Clause 7.1 requires cooling below 1000 F [538 C] after hot working before heat treating.
No. Clause 7.3.1 offers that route to many austenitic grades but names F310H among the exclusions, alongside F304H, F309H, F310, F316H, F321, F321H, F347, F347H, F348, F348H, F45 and F56. A separate solution anneal and liquid quench is required.
ASTM No. 6 or coarser, determined to Test Methods E112. Grades F304H, F309H, F310H and F316H all carry this requirement. Coarse grain reduces the grain-boundary area available for creep deformation, which is the purpose of an H grade.
No. Clause 6.4.1 prohibits machining flanges of any type, elbows, return bends, tees and header tees directly from bar stock. Cylindrically shaped parts may be machined from forged or rolled solution-annealed austenitic bar without additional hot working, but flanges must be forged.
A182 itself caps products at 10 000 lb, 4540 kg, and refers heavier austenitic parts to A965/A965M. Plant capacity reaches 30,000 kg on a single piece, set by the 60 t heat size and the 6,300 t press, with rings to OD 6,000 mm and shafts to 14,000 mm turned length.
It is not designed for it. The high carbon that gives the grade its creep strength is detrimental to aqueous corrosion resistance, and the alloy becomes prone to intergranular corrosion after prolonged high-temperature exposure. For wet corrosive duty, 904L, Sanicro 28 or a nickel alloy such as Hastelloy C-276 is the better choice.
Two. Continuous service between 425 and 860 C is not advised because of carbide precipitation. Sigma phase precipitates on holding between 650 and 950 C, and a solution anneal at 1100 to 1150 C restores a degree of toughness. Frequent thermal cycling also reduces oxidation resistance.
Frequently, yes, since the carbon range and grain size of a given lot can satisfy both sets of requirements at once. That is a property of the heat rather than a general equivalence. Where creep strength governs, order S31009 and require carbon and grain size results on the certificate.
Ultrasonic testing to EN 10228-4, the part covering austenitic and austenitic-ferritic stainless forgings, with ASTM A388/A388M or SEP 1921 as alternatives. Inspection documents to EN 10204 Type 3.1, or Type 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector. A262 or G28 intergranular corrosion testing is placed with an accredited third-party laboratory.
Data on this page is compiled from the standards and published data sheets listed above and is given for information. It is not a guarantee and not an express or implied warranty of suitability for any application. Material selection and code allowable stresses remain the responsibility of the purchaser's design engineer. Page last reviewed 5 October 2026.
Send a drawing, or the outside diameter, inside diameter, height and quantity. State the governing specification, A182 F310H or A965 F310H, the delivery condition, the certificate type, EN 10204 3.1 or 3.2, and any ultrasonic acceptance class, and the price will be firm rather than indicative. Minimum order 10 kg with no minimum piece count. Lead time 20 to 60 days.