UNS S30909 Forgings ASTM A182 F309H seamless rolled rings, flanges, discs, shafts and bars in 22Cr 13Ni heat-resisting stainless steel
UNS S30909 is the Unified Numbering System number for 309H austenitic heat-resisting stainless steel. It holds 22.0 to 24.0 per cent chromium, 12.0 to 15.0 per cent nickel and a controlled carbon band of 0.04 to 0.10 per cent. That band sits above the 0.08 per cent ceiling of 309S because carbon raises creep strength at temperature. Forged, the grade is ordered to ASTM A182 or ASME SA-182 Grade F309H, with a minimum tensile strength of 515 MPa (75 ksi) and a minimum yield strength of 205 MPa (30 ksi).
309H is a high-temperature oxidation grade, not a wet-corrosion grade. It resists oxidation to roughly 1038 C (1900 F) in non-cyclic service.
Jiangyin Jiangnan Metal melts S30909 in its own electric arc furnace, refines it in the ladle and under vacuum, then forges or ring-rolls it on site. Rings roll to 6,000 mm outside diameter and single pieces run to 30 tonnes. Minimum order is 10 kg with no minimum piece count.
- UNS
- S30909
- Also called
- 309H, SS 309H, Type 309H
- Forging spec
- ASTM A182 / SA-182 F309H
- Chromium
- 22.0 to 24.0 %
- Nickel
- 12.0 to 15.0 %
- Carbon
- 0.04 to 0.10 %
- Tensile min
- 515 MPa / 75 ksi
- Yield min
- 205 MPa / 30 ksi
- Oxidation
- to 1038 C non-cyclic
- Ring size
- OD 50 to 6,000 mm
- Piece weight
- 10 kg to 30,000 kg
- Certification
- EN 10204 3.1 or 3.2
- Enquiries
- sales@steelforgepieces.com
+86 189 2135 9659
On this page
Designations by product form
309H carries a different grade mark in every product specification. The row that governs the parts on this page is the first one. The others are listed because buyers routinely cross-reference a plate or pipe grade when ordering a matching forging.
| Product form | Specification | Grade mark |
|---|---|---|
| Forgings, flanges, fittings, valves | ASTM A182 / ASME SA-182 | F309H (S30909) |
| Plate, sheet, strip | ASTM A240 / ASME SA-240 | 309H (S30909) |
| Seamless and welded pipe | ASTM A312 | TP309H |
| Seamless tube | ASTM A213 | TP309H |
| Plate, sheet, strip, 309 family | AMS | 5523 |
| European near-equivalent | EN 10095 | 1.4833, X12CrNi23-13 |
EN 1.4833 is normally cross-referenced to 309 and 309S rather than to the H-grade carbon band, so treat it as a near-equivalent and not a drop-in substitute. Where a design calculation relies on H-grade allowable stresses, order to A182 F309H or A240 309H by name.
Chemical composition
Two sets of limits circulate for S30909 and they differ on silicon. The forging specification allows 1.00 per cent maximum. The plate specification holds it to 0.75 per cent. If your drawing quotes the plate limit, state it on the order and the heat will be aimed at the tighter band.
| Element | ASTM A182 F309H, forgings | ASTM A240 309H, plate |
|---|---|---|
| Carbon, C | 0.04 to 0.10 | 0.04 to 0.10 |
| Chromium, Cr | 22.0 to 24.0 | 22.0 to 24.0 |
| Nickel, Ni | 12.0 to 15.0 | 12.0 to 15.0 |
| Manganese, Mn | 2.00 | 2.00 |
| Silicon, Si | 1.00 | 0.75 |
| Phosphorus, P | 0.045 | 0.045 |
| Sulphur, S | 0.030 | 0.030 |
| Iron, Fe | Balance | Balance |
S30909 is not a stabilised grade
No niobium or titanium addition appears in the composition of UNS S30909. Its strength at temperature comes from carbon. Where an application genuinely needs a niobium-stabilised austenitic forging, the grades to specify are ASTM A182 F347 and F347H, UNS S34700 and S34709. For titanium stabilisation, use F321 or 321H. All of these are forged here. Several published grade sheets describe 309H as niobium stabilised, which is where the confusion starts.
Mechanical properties
Acceptance minima differ between the forging and the plate specification. Elongation is 30 per cent minimum for A182 F309H forgings against 40 per cent for A240 309H plate, and forgings additionally carry a reduction-of-area requirement that plate does not.
| Property | A182 F309H, forgings | A240 309H, plate |
|---|---|---|
| Tensile strength, min | 515 MPa / 75 ksi | 515 MPa / 75 ksi |
| Yield strength 0.2 % offset, min | 205 MPa / 30 ksi | 205 MPa / 30 ksi |
| Elongation in 50 mm or 4D, min | 30 % | 40 % |
| Reduction of area, min | 50 % | not specified |
| Hardness, max | by order or supplementary requirement | 217 HBW |
| Yield 0.2 % offset | Tensile | Elongation in 50 mm | Hardness |
|---|---|---|---|
| 310 MPa / 45,000 psi | 586 MPa / 85,000 psi | 50 % | 202 HBN |
Typical values are indicative and must not be used as design allowables. Design to the specified minima and to the allowable stresses in ASME BPVC Section II Part D.
Physical properties
| Property | Metric | Imperial |
|---|---|---|
| Density | 7.89 g/cm3 | 0.285 lb/in3 |
| Modulus of elasticity | 193 GPa | 28.5 x 106 psi |
| Melting range | 1480 to 1530 C | 2500 to 2590 F |
| Specific heat | 502 J/kg·K, 0 to 100 C | 0.12 BTU/lb·F, 32 to 212 F |
| Thermal conductivity | 15.6 W/m·K at 100 C | 9.0 BTU/hr/ft2/ft/F at 212 F |
| Electrical resistivity | 78 microhm·cm at 20 C | 30.7 microhm·in at 68 F |
| Magnetic response | Essentially non-magnetic in the annealed austenitic condition | |
Creep and creep rupture
Creep is the reason 309H exists as a grade separate from 309S. The figures below are typical published data for the 309 family and show how quickly load-bearing capacity falls away above 700 C. For a furnace ring, a tube hanger or a walking beam, this table decides the section thickness long before the oxidation limit does.
| Temperature | Creep strain | Creep rupture | ||||
|---|---|---|---|---|---|---|
| 1,000 h | 10,000 h | 100,000 h | 1,000 h | 10,000 h | 100,000 h | |
| 600 C / 1112 F | 120 | 80 | 40 | 190 | 120 | 65 |
| 700 C / 1292 F | 50 | 25 | 20 | 75 | 36 | 16 |
| 800 C / 1472 F | 20 | 10 | 8 | 35 | 18 | 7.5 |
| 900 C / 1652 F | 8 | 4 | 3 | 15 | 8.5 | 3 |
| 1000 C / 1832 F | 4 | 2.5 | 1.5 | 8 | 4 | 1.5 |
Typical data for guidance. Design to the governing pressure vessel or piping code.
Service temperature limits by atmosphere
309H works because 23 per cent chromium builds a protective oxide scale. What the furnace atmosphere does to that scale matters as much as the temperature reading, so the limits are quoted by atmosphere rather than as a single number.
| Condition | Limit |
|---|---|
| Oxidation resistance, non-cyclic | 1038 C / 1900 F |
| Oxidation resistance, frequent thermal cycling | about 1010 C / 1850 F |
| Oxidising, sulphur to 2 g/m3, continuous | 1050 C / 1922 F |
| Oxidising, sulphur to 2 g/m3, peak | 1100 C / 2012 F |
| Oxidising, sulphur above 2 g/m3 | 950 C / 1742 F maximum |
| Low oxygen atmosphere, sulphur to 2 g/m3 | 1000 C / 1832 F maximum |
| Nitriding or carburising atmospheres | 850 to 950 C / 1562 to 1742 F maximum |
Two behaviours need designing around. The alloy precipitates sigma phase when held between 650 and 950 C, which embrittles it, and a solution anneal at 1100 to 1150 C restores a degree of toughness. It also shows only moderate resistance to carbon absorption, so it is not recommended for highly carburising atmospheres. In reducing, nitriding and carburising service it outperforms most heat-resisting stainless steels but does not match Alloy 600 or Alloy 800.
Forging, heat treatment, machining
Melting
S30909 is melted in the 25 t electric arc furnace, refined in a ladle furnace and decarburised under vacuum in the 30 t or 60 t VOD unit, which is where the carbon band is brought inside 0.04 to 0.10 per cent and held there. Maximum heat size is 60 tonnes. Electroslag remelting is available where an order calls for improved cleanliness. The melt route is recorded on the certificate.
Hot forging
Heat uniformly and work between 950 and 1200 C (1742 to 2192 F). Reheat rather than carry on below the bottom of that range. After hot forming, a final anneal at 1000 to 1150 C (1832 to 2101 F) with rapid quenching is recommended. Where the piece has sat in the sigma range, solution anneal at 1100 to 1150 C.
Cold forming
The alloy is quite ductile and forms in a manner very similar to 316. Cold forming is not recommended for pieces that will see long-term exposure to high temperature, because the alloy is subject to carbide and sigma phase precipitation.
Machining
Treat S30909 as a work-hardening austenitic. Rigid setups, sharp tooling, positive rake, generous coolant, constant feed, no dwell. Rough machining normally follows the solution anneal, with finish machining afterwards. Parts can leave as-forged with allowance, proof-machined for ultrasonic inspection, or finish-machined to drawing.
Welding
The 309 family welds readily by TIG, plasma, MIG, SMAW, SAW and FCAW. Where the best corrosion resistance after welding is wanted, the low-carbon 309S variant is preferred because it limits carbide precipitation. That trade-off is worth weighing when an H-grade forging is going to be welded into an assembly.
Forged shapes in UNS S30909
Everything below is forged from steel melted on this site, to customer drawing or sample. No casting, no welded fabrication, no purchased billet of unknown origin.
Seamless rolled rings
Ring-rolled from a punched preform on the radial-axial mills, rectangular or contoured section, outside diameter 50 to 6,000 mm. Grain flow follows the circumference, which is what furnace retort flanges and bearing housings want.
Forged flanges
Weld neck, blind, slip-on, socket weld, lap joint, orifice, long weld neck and special-bore flanges to ASME B16.5 and B16.47 patterns, covered by ASTM A182.
Discs, tube sheets, covers
Upset-forged discs and tube sheets for recuperators and heat exchangers, machined to 5,000 mm diameter on the vertical lathes and supplied proof-machined for volumetric inspection.
Shafts and spindles
Stepped shafts, eccentric shafts and spindles for furnace fans, kiln drives and hot rotating equipment. Turned to 14 m between centres, quenched vertically in the 15 m well furnaces.
Sleeves, bushings, hollow bar
Bored and trepanned hollows, liners, couplings and sleeves to 1,600 mm diameter by 10,000 mm on the deep-hole drilling machine.
Bars and blocks
Forged round, flat and square bar plus blocks, cut to length, as feedstock for machined valve bodies and furnace hardware.
Valve and wellhead parts
Bodies, bonnets, blocks, stems, seat rings, spools and nozzles for ball, gate, globe, check and plug valves in hot service.
Gear and wheel blanks
Gear ring blanks, retaining rings, slewing rings, crane wheels and pinion blanks for drives running at temperature.
Custom open-die work
Stepped cylinders, forged rolls and non-standard profiles. Send a drawing and the nearest economical forging envelope will be quoted.
Works capability for this grade
Most forging suppliers in China buy billet. This plant starts at the furnace, so the chemistry of an S30909 heat can be aimed at the forging it will become rather than accepted as delivered, and traceability runs from the melt number through to the shipped part.
| Item | Figure | Set by |
|---|---|---|
| Melting route for stainless | EF, LF, VOD. ESR where cleanliness governs | 25 t arc furnace, 25 and 50 t ladle furnaces, 30 and 60 t VOD |
| Maximum heat | 60 t | VOD vessel |
| Seamless rolled rings | OD 50 to 6,000 mm | 6 m, 3 m and 1 m radial-axial mills; upset-and-punch below mill range |
| Heaviest single forging | 30,000 kg | 6,300 t press, backed by 4,000 t and 2,000 t |
| Machined disc diameter | to 5,000 mm | 5,000 mm vertical turning lathe |
| Shaft length | to 14,000 mm turned | C61160 horizontal lathe, 15 m well furnaces for vertical quench |
| Bored cylinders | to 1,600 mm dia x 10,000 mm | CNC deep-hole drilling machine |
| Solution annealing | 1100 to 1150 C | 14 furnaces, including 3 high-temperature car-bottom units |
| Minimum order | 10 kg, no minimum piece count | Weight-based, not quantity-based |
| Lead time | 20 to 60 days | Shorter without a remelting step, longer with one |
| Class approvals | CCS, BV, DNV, LR, NK | Works approvals |
Where S30909 forgings are used
The application set follows the property profile: sustained high temperature, oxidising or moderately sulphidising atmospheres, and load-bearing duty where creep governs the design.
| Sector | Components |
|---|---|
| Industrial furnaces | Burners, doors, fan hubs and shafts, piping, recuperators |
| Fluidised bed furnaces | Grids, piping, wind boxes |
| Thermal processing | Annealing covers and boxes, burner grids, muffles and retorts, lead pans and neutral salt pots, walking beams, fans |
| Petroleum refining | Catalytic recovery systems, recuperators |
| Power generation | Pulverised coal burners, tube hangers and supports |
| Waste treatment | Incinerator parts, rotary kilns, calciners |
| Pulp and paper | Paper mill equipment running hot |
When not to specify 309H
Not a wet corrosion grade
Alloy 309 is not designed for service in wet corrosive environments. The high carbon content that improves creep properties has a detrimental effect on aqueous corrosion resistance, and the alloy is prone to intergranular corrosion after long-term exposure at high temperature. Its 23 per cent chromium does make it more corrosion resistant than most heat-resisting alloys, but that is a comparison inside the heat-resisting family, not a case for seawater or process acid duty.
| Requirement | Grades to consider |
|---|---|
| Seawater, subsea, chloride-rich service | F51, F53, F55, F44, 904L |
| Hot service with heavy welding, stabilisation wanted | F347 and F347H, F321 and 321H |
| Fabrication-led assembly, best weldability | 309S, UNS S30908, low-carbon variant |
| Carburising or strongly reducing atmospheres | Alloy 800H and 800HT, Alloy 600, Alloy 602 CA, Alloy 45TM |
| Continuous service above 1050 C | Haynes 230, Inconel 617, AISI 330 |
| Hygienic or food-contact service | F316L, F304L |
Testing and certification
Testing runs in the works laboratory. Because the steel is melted here, chemistry is verified at the furnace rather than taken from a supplier certificate.
| Discipline | Standard | Where |
|---|---|---|
| Chemical analysis, optical emission | ASTM E415 | On site |
| Carbon and sulphur, infrared | ASTM E1019 | On site |
| Positive material identification | Handheld analyser | On site |
| Tensile testing | ASTM A370, ISO 6892 | On site, 600 kN and 300 kN machines |
| Ultrasonic testing | ASTM A388, EN 10228-3 | On site |
| Magnetic particle inspection | ASTM E709 | On site |
| Grain size | ASTM E112 | On site |
| Hardness | ASTM A956, converted per ASTM E140 | On site |
| Intergranular corrosion | ASTM A262 | Accredited third-party laboratory |
| Bench Brinell or Rockwell hardness | Where the specification requires a bench machine | Accredited third-party laboratory |
| Mill certificate | EN 10204 3.1 | Standard |
| Witnessed certificate | EN 10204 3.2 | BV, DNV, LR, SGS, TUV or customer inspector |
Supporting records include heat-treatment charts, NDT reports, dimensional reports and PMI records. Flag witnessed inspection and outside laboratory testing at enquiry stage so they are built into the quoted date rather than added to it.
Questions about UNS S30909
What is UNS S30909?
UNS S30909 is the Unified Numbering System number for 309H austenitic heat-resisting stainless steel, holding 22.0 to 24.0 per cent chromium, 12.0 to 15.0 per cent nickel and 0.04 to 0.10 per cent carbon. The carbon band is higher than that of 309S because carbon raises creep strength at temperature. Forged, the grade is ordered to ASTM A182 or ASME SA-182 Grade F309H.
What is the difference between 309, 309S and 309H?
All three share the same 22 to 24 per cent chromium and 12 to 15 per cent nickel base, and only carbon changes. Alloy 309, UNS S30900, allows up to 0.20 per cent. Alloy 309S, UNS S30908, is the low-carbon version at 0.08 per cent maximum for ease of fabrication and better weldability. Alloy 309H, UNS S30909, carries a controlled 0.04 to 0.10 per cent band for improved creep resistance. In many heats the grain size and carbon content satisfy both the 309S and the 309H requirements at once, so dual-certified material is common.
Is UNS S30909 niobium stabilised?
No. S30909 specifies no niobium or titanium addition and is not a stabilised grade. Its strength at temperature comes from carbon. The niobium-stabilised austenitic grades are 347 and 347H, forged to ASTM A182 F347 and F347H. The titanium-stabilised grades are 321 and 321H. This point is worth confirming on the purchase order, because several published grade sheets state it incorrectly.
What is the maximum service temperature of 309H forgings?
About 1038 C (1900 F) for oxidation resistance in non-cyclic conditions, falling to roughly 1010 C (1850 F) where thermal cycling is frequent. In oxidising conditions with sulphur up to 2 g/m3 the rating is 1050 C continuous with a 1100 C peak. Above 2 g/m3 sulphur the limit is 950 C. In a low-oxygen atmosphere with sulphur up to 2 g/m3 it is 1000 C. In nitriding or carburising atmospheres the maximum is 850 to 950 C, and the grade is not recommended for highly carburising service. Creep governs load-bearing capacity well below all of these figures.
How is UNS S30909 heat treated after forging?
Hot work uniformly between 950 and 1200 C. After hot forming, anneal at 1000 to 1150 C and quench rapidly. If the part has been held between 650 and 950 C and sigma phase has precipitated, a solution anneal at 1100 to 1150 C restores a degree of toughness.
Can 309H be used in wet corrosive service?
It should not be selected for that duty. Alloy 309 is not designed for wet corrosive environments. The high carbon content present to improve creep properties has a detrimental effect on aqueous corrosion resistance, and the alloy is prone to intergranular corrosion after long-term high-temperature exposure. For seawater, subsea and chloride-rich service, specify duplex or super-duplex forgings such as F51, F53 and F55, or super-austenitic grades such as F44 and 904L.
What size S30909 forgings can you produce?
Seamless rings roll to 6,000 mm outside diameter on the 6 m radial-axial mill, with 3 m and 1 m mills for smaller sizes and an upset-and-punch route from 50 mm outside diameter. The heaviest single forging is 30 tonnes, worked on 6,300 t, 4,000 t and 2,000 t presses. Vertical lathes machine to 5,000 mm swing, horizontal lathes to 14 m between centres, and the deep-hole drilling machine bores 1,600 mm diameter by 10,000 mm. Minimum order is 10 kg with no minimum piece count.
Do you melt your own S30909, or buy billet?
It is melted here. Stainless grades run through the 25 t electric arc furnace, are refined in 25 t and 50 t ladle furnaces and decarburised under vacuum in 30 t and 60 t VOD units, with 60 tonnes the maximum heat size. Electroslag remelting is available where cleanliness governs. Because melting is on site, the certificate traces a part back to its melt number instead of stopping at a purchased billet certificate.
What certification comes with the forgings?
EN 10204 3.1 mill test certificates as standard, or 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector. Ultrasonic testing to ASTM A388 and EN 10228-3, magnetic particle to ASTM E709, grain size to ASTM E112 and PMI are run in the works laboratory. Intergranular corrosion testing to ASTM A262 is placed with an accredited third-party laboratory and reported alongside the mill certificate.
How do I request a quotation?
Six items cover it: the grade or specification, for example ASTM A182 F309H; the dimensions or a drawing in PDF, DWG, DXF or STEP; the quantity and expected repeat volume; the delivery condition, as-forged, proof-machined or finish-machined; the heat treatment and testing requirements; and the certification and destination port. Every forging is made to order, so prices are quoted against the drawing rather than listed. If the grade is still open, send the operating temperature and the atmosphere and the choice can be confirmed before pricing.
Enquiry
Send a drawing or a written specification. Quotations normally come back within two working days. If a different grade suits the service better, that will be said plainly before a price is given.
- Manufacturer
- Jiangyin Jiangnan Metal Co., Ltd.
Integrated melting works and open-die forge, since 1997 - Plant
- No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
- Telephone, WhatsApp, WeChat
- +86 189 2135 9659
- Hours
- Monday to Saturday, 08:00 to 17:30 China Standard Time, UTC+8
- Documentation
- EN 10204 3.1 and 3.2. CCS, BV, DNV, LR, NK approvals
Related grades forged here
- AISI 347H
- AISI 321H
- A182 F347
- A182 F321
- AISI 330
- A182 F316
- A182 F316L
- A182 F44
- A182 F51
- A182 F53
- A182 F55
- 904L
- Incoloy 800H
- Inconel 617
- Haynes 230
Reviewed by the technical sales department, Jiangyin Jiangnan Metal Co., Ltd. Property data compiled from published mill data sheets and from ASTM A182 and ASTM A240. Given for information. Design to the current issue of the governing code and confirm requirements on the purchase order.