UNS N08033 (R20033 / Alloy 33 / 1.4591) Forgings
Published by Jiangyin Jiangnan Metal Co., Ltd. Last reviewed 4 October 2026. Data from ASTM B462, B625 and B649, VDM Metals Data Sheet No. 4142 and Koehler et al., NACE CORROSION 96.
UNS N08033 and UNS R20033 are the same material: Alloy 33, also sold as Nicrofer 3033 and designated W.Nr. 1.4591. It is a nitrogen-alloyed high-chromium austenitic stainless steel with nominally 33 % chromium, 31 % nickel, 32 % iron, 1.6 % molybdenum, 0.6 % copper and 0.4 % nitrogen.
ASTM and ASME specifications use R20033. N08033 survives as a secondary listing in supplier catalogues and older cross-reference tables. On a purchase order or a material specification, write UNS R20033 plus the ASTM number, and show N08033 only as an equivalent.
We forge this grade to order as round bar, seamless rolled rings, flanges, discs, blocks, hollow bars and sleeves to ASTM B462, ASTM B649 and customer drawings, supplied solution annealed with EN 10204 3.1 or 3.2 certificates.
Full datasheet, including elevated-temperature strength, physical property tables, corrosion rates in sulphuric, phosphoric and nitric-hydrofluoric acid, welding parameters and grade comparisons: 1.4591 / Alloy 33 / UNS R20033 forgings
- ASTM and ASME UNS
- R20033
- Secondary listing
- N08033
- W.Nr.
- 1.4591
- Trade names
- Alloy 33, Nicrofer 3033
- Rp0.2 minimum
- 380 MPa
- Rm at 20 °C
- 720 to 920 MPa
- Elongation minimum
- 40 %
- Hardness
- 240 HBW max
- PREN with 16N
- 44.7
- Density
- 7.90 g/cm³
- Melting range
- 1330 to 1370 °C
- Service range
- −196 to 450 °C
N08033 or R20033: which number belongs on the order
The alloy was introduced in 1995 by Krupp VDM, now VDM Metals. Its Unified Numbering System assignment falls in the R series rather than the N series because iron is the balance of the composition at roughly 32 %, which classifies it as a chromium-based austenitic stainless steel rather than a nickel alloy. Every current ASTM specification containing the grade uses R20033.
N08033 still appears in distributor catalogues and cross-reference tables, usually printed next to R20033. It describes the same chemistry and the same properties, so a request for either is filled from the same material. The risk is documentary rather than metallurgical. A certificate stamped only N08033 can be queried by an inspector checking against ASTM B462 or B649, which name R20033. Our certificates show UNS R20033, also listed as N08033, together with 1.4591 and Alloy 33, so both readings are covered.
Designation set: UNS R20033, UNS N08033, W.Nr. 1.4591, EN name X1CrNiMoCuN33-32-1 (also written X1NiCrMoCuN 33-32-1), Alloy 33, Nicrofer 3033, GB NS1405.
Chemical composition
| Element | Symbol | Minimum | Maximum | Nominal |
|---|---|---|---|---|
| Chromium | Cr | 31.0 | 35.0 | 33 |
| Nickel | Ni | 30.0 | 33.0 | 31 |
| Iron | Fe | Balance | 32 | |
| Molybdenum | Mo | 0.5 | 2.0 | 1.6 |
| Nitrogen | N | 0.35 | 0.60 | 0.4 |
| Copper | Cu | 0.3 | 1.2 | 0.6 |
| Manganese | Mn | – | 2.00 | – |
| Silicon | Si | – | 0.50 | – |
| Carbon | C | – | 0.015 | 0.010 |
| Phosphorus | P | – | 0.020 | – |
| Sulphur | S | – | 0.010 | – |
Carbon is held below 0.015 % to limit chromium carbide precipitation at grain boundaries. Nitrogen between 0.35 and 0.60 % keeps the structure fully austenitic, lifts minimum proof strength to 380 MPa, and contributes a large share of the pitting resistance.
Specifications by product form
| Product form | ASTM | ASME |
|---|---|---|
| Forged flanges, fittings, valves and parts | B462 | SB-462 |
| Bar, rod, wire and forging stock | B649 | SB-649 |
| Plate, sheet and strip | B625 | SB-625 |
For forged components the governing specification is normally ASTM B462, which covers forged or rolled pipe flanges, forged fittings, valves and parts in R20033 for corrosive high-temperature service. ASTM B649 is titled for Ni-Fe-Cr-Mo-Cu-N low-carbon alloys and Cr-Ni-Fe-N low-carbon alloy, with R20033 in the second group. No direct GB/T national equivalent exists, so material sourced in China is supplied against the ASTM or EN designation.
Mechanical and physical properties
| Property | Metric | Imperial |
|---|---|---|
| 0.2 % proof strength Rp0.2 | 380 MPa minimum | 55.1 ksi minimum |
| Tensile strength Rm | 720 to 920 MPa | 104 to 133 ksi |
| Elongation A | 40 % minimum | 40 % minimum |
| Brinell hardness | 240 HBW maximum | 240 HBW maximum |
| Density | 7.90 g/cm³ | 0.285 lb/in³ |
| Melting range | 1330 to 1370 °C | 2426 to 2498 °F |
| Structure | Face-centred cubic, fully austenitic | |
| Approved service range | −196 to 450 °C | −320 to 842 °F |
Minimum proof strength is roughly double that of AISI 316L at room temperature, which often permits thinner walls and lighter forgings at the same design pressure.
Why 33 % chromium instead of more molybdenum
Most high-performance austenitic stainless steels buy corrosion resistance with molybdenum, up to 6 % in the super-austenitic grades. This alloy takes the other route, and that changes where it wins.
In strongly oxidising media the passive film built on 33 % chromium holds where molybdenum-rich alloys are attacked, which is why the grade is specified for hot concentrated sulphuric acid, nitric acid and nitric-hydrofluoric mixtures. In reducing acids the logic reverses and a molybdenum-rich grade such as Alloy 31 or a nickel-base alloy is the better selection. The 1.6 % molybdenum addition improves behaviour in phosphoric acid and the 0.6 % copper assists passivation in sulphuric acid.
For chloride pitting the nitrogen carries the load:
PREN = Cr + 3.3 Mo + 16 N = 33 + 5.28 + 6.4 = 44.7
PREN = Cr + 3.3 Mo + 30 N = 33 + 5.28 + 12.0 = 50.3
Both formulas are in use. The 16N version is the conservative one normally quoted in specifications. Seawater service typically calls for PREN above 40, which the grade clears either way. Because chemistry varies inside the specified limits, recalculate from the heat analysis on the certificate rather than from nominal values.
One operating condition overrides all of it. Full corrosion resistance is reached only when the surface is clean and metallically bright. Forging scale, grinding burn, embedded iron and weld heat tint all reduce it. Every forging we ship in this grade is solution annealed and descaled, and pickled where specified.
Applications
| Service | Application | Forgings required |
|---|---|---|
| Sulphuric acid production | Heat recovery and acid distribution systems, heat exchangers on acid carrying chlorides | Flanges, tubesheets, valve bodies, blocks |
| Nitric and mixed acid | Nitric-hydrofluoric pickling plant, acid storage and transport | Rings, flanges, nozzles, hollow bars |
| Seawater and brackish water | Seawater piping, plate and tubular heat exchangers using seawater as coolant | Rolled rings, flanges, pump shafts, sleeves |
| Caustic service | Production and handling of sodium hydroxide | Flanges, discs, valve internals |
| Pulp and paper | Bleaching plant for chemical pulp | Rings, shafts, sleeves |
Forging and heat treatment
The grade takes open-die forging and ring rolling well, but the window is narrower than for standard austenitic stainless steels and the post-forge heat treatment is not optional. This is the sequence we run in Jiangyin.
Cleanliness before heating
Billets must be free of sulphur, phosphorus, lead and other low-melting metals, which embrittle the alloy at forging temperature. These reach the workpiece through marking paint, temperature crayons, grease, oil and fuel. Electric furnaces are preferred because they add no combustion products and hold temperature more tightly.
Furnace atmosphere
Keep the atmosphere neutral to slightly oxidising, avoid swinging between oxidising and reducing, and keep flame off the workpiece.
Hot forging
Charge into a furnace already at temperature, around 1200 °C maximum, and forge between 1200 and 1000 °C. Do not finish below 1000 °C. The alloy is strong hot and work-hardens quickly, so low finishing temperatures invite cracking. Cool quickly after forging.
Solution annealing
Solution anneal at 1100 to 1150 °C, charging into a furnace already at temperature, then water quench. Soak time is counted from the moment the section reaches temperature and scales with thickness per the mill data sheet. Over-soaking does far less harm than under-soaking.
Machining and welding
Machine from the solution-annealed condition at low cutting speed and moderate feed, with continuous tool engagement and enough depth of cut to work under the strain-hardened layer. A tool that dwells leaves a hardened skin for the next pass. Weld with a matching filler, stringer beads and low heat input. High nitrogen makes the weld pool prone to porosity, and thin beads give it time to degas. Post-weld heat treatment is normally not required.
Forged products and sizes
We are a forging factory, not a stockist reselling mill product. This grade is forged to order from certified billet, solution annealed in our own furnaces, machined to drawing where required, and tested before release.
| Product form | Size range | Notes |
|---|---|---|
| Round bar, rods, shafts | 80 to 1200 mm diameter, up to 6000 mm long | Turned, peeled or black, step shafts to drawing |
| Square, rectangular, flat, hex bar | 30 to 800 mm thickness | Saw cut to length |
| Seamless rolled rings | 200 to 3500 mm outside diameter, 30 to 500 mm wall, up to 1000 mm height | Rectangular or profiled section |
| Forged flanges | DN 15 to DN 2000, up to Class 2500 | Weld neck, slip-on, blind, lap joint, orifice, special |
| Discs, blanks, plates | 100 to 2500 mm diameter, 20 to 600 mm thick | Tubesheets, blind discs, cover plates |
| Hollow bars, sleeves, bushes, cylinders | 120 to 1500 mm outside diameter, bore from 60 mm | Trepanned or expanded, bored and honed on request |
| Blocks, hubs, housings, casings, barrels | Up to 8000 kg single piece | Valve bodies and custom forgings to drawing |
Standard delivery condition is forged, solution annealed, water quenched and descaled, with surface black as forged, rough machined, or finish machined to drawing tolerance. Rough-machined parts normally carry 6 to 12 mm allowance per side. Marking is hard stamped or low-stress vibro marked with grade, heat number, order number and specification, using sulphur-free and chloride-free media.
Testing and certification
| Category | Scope |
|---|---|
| Chemical analysis | Full spectro analysis per heat including N, C and S, with PREN calculated per heat on request |
| Mechanical testing | Tensile, Brinell hardness and Charpy V-notch impact at room or low temperature |
| Non-destructive testing | Ultrasonic, dye penetrant and dimensional inspection, radiography on request |
| Corrosion testing | Intergranular corrosion to ASTM A262 practice C or customer specification |
| Heat treatment records | Calibrated furnace charts with charge, soak and quench data for each lot |
| Certification | EN 10204 3.1 as standard, 3.2 with third-party witness on request |
Questions
Is UNS N08033 the same as UNS R20033?
Yes. Both refer to Alloy 33, W.Nr. 1.4591, with nominally 33 % Cr, 31 % Ni, 32 % Fe, 1.6 % Mo, 0.6 % Cu and 0.4 % N. ASTM B462, B625 and B649 use R20033. N08033 appears as a secondary listing in supplier literature. Quote R20033 plus the ASTM number on orders and certificates.
Is it a stainless steel or a nickel alloy?
By composition it is an austenitic stainless steel, since iron is the balance at about 32 %, which is why it carries an R-series UNS number. With 31 % nickel it sits at the boundary with the nickel-iron-chromium alloys and is specified in ASTM standards alongside them, but it is bought, forged and fabricated like a super-austenitic stainless steel.
Which specification applies to forgings?
ASTM B462 and ASME SB-462 for forged flanges, fittings, valves and parts. ASTM B649 and ASME SB-649 for bar and wire, which covers forging stock. ASTM B625 and ASME SB-625 for plate, sheet and strip.
What is the forging temperature range?
Forge between 1200 and 1000 °C, charging into a furnace already at temperature, then cool rapidly. Do not finish below 1000 °C. A solution anneal at 1100 to 1150 °C with a water quench follows to restore full corrosion resistance.
What is the PREN?
44.7 using Cr plus 3.3 Mo plus 16 N on the nominal analysis, or 50.3 using the 30 N formula. Both clear the value of 40 normally required for seawater. Recalculate from the actual heat analysis for design work.
Is the grade held in stock?
No. It is forged to order rather than held as general stock, normally within 25 to 40 days depending on size and testing scope. Send a drawing, or the form, dimensions, quantity, specification and test requirements.
What are the alternative grades?
Alloy 31 and 1.4562 for reducing acids and phosphoric acid, UNS S31254 and 1.4529 for chloride service, and 904L for milder sulphuric and phosphoric duty. In strongly oxidising service none of these matches R20033, because its resistance comes from 33 % chromium rather than from molybdenum. Comparison on the 1.4591 page.
Request a quotation for UNS N08033 forgings
Send a drawing, or just the form, dimensions, quantity and specification. Technical enquiries are answered within one working day with weight, lead time and price.
Cite this page
Jiangyin Jiangnan Metal Co., Ltd. (2026). UNS N08033 (R20033 / Alloy 33 / 1.4591) Forgings. Jiangyin, Jiangsu, China. https://www.steelforgepieces.com/Stainless-Steel/UNS-N08033.html
References
- ASTM B649, Standard Specification for Ni-Fe-Cr-Mo-Cu-N Low-Carbon Alloy and Cr-Ni-Fe-N Low-Carbon Alloy (UNS R20033) Bar and Wire.
- ASTM B462, Standard Specification for Forged or Rolled Alloy Pipe Flanges, Forged Fittings, and Valves and Parts for Corrosive High-Temperature Service.
- ASTM B625, Standard Specification for Plate, Sheet and Strip.
- VDM Metals International GmbH, VDM Alloy 33, Material Data Sheet No. 4142.
- M. Koehler, U. Heubner, K. W. Eichenhofer, M. Renner, Progress with Alloy 33 (UNS R20033), a New Corrosion-Resistant Chromium-Based Austenitic Material, CORROSION 96, Paper 428, NACE International, 1996.
Data is published for engineering guidance and is not a guarantee of properties in a specific application. Material selection for a given service environment remains with the purchaser. Trade names belong to their respective owners. Jiangyin Jiangnan Metal Co., Ltd. is not affiliated with VDM Metals.