Z7CND18-12-03 Forgings: AFNOR Grade, EN 1.4436 / X3CrNiMo17-13-3
Forged rings, seamless rolled rings, flanges, shafts, discs, tube sheets and valve parts in Z7CND18-12-03, melted and forged in one works.
Z7CND18-12-03, also written Z7CND18.12.03 or Z7CND18-12-3, is the French AFNOR designation from standard NF A 35-574 for an austenitic chromium-nickel-molybdenum stainless steel. Its European equivalent is EN 1.4436 / X3CrNiMo17-13-3, and it cross-references to AISI 316 (UNS S31600), JIS SUS316 and BS 316S33.
The Z7 in the designation stands for roughly 0.07 % carbon. This is a standard carbon grade in the 316 family, not a low carbon or nitrogen alloyed one. What separates it from ordinary 1.4401 / 316 is the molybdenum range of 2.5 to 3.0 %, which raises resistance in chloride bearing and acid media.
Jiangyin Jiangnan Metal Co., Ltd. produces Z7CND18-12-03 open-die forgings and seamless rolled rings from steel melted on its own site in Jiangyin, Jiangsu, China, up to 6,000 mm ring outside diameter and 30 tonnes single-piece weight, minimum order 10 kg, with EN 10204 3.1 or 3.2 certification.
International equivalents and standards
Z7CND18-12-03 appears in French practice and in older multinational drawing packages. When a customer specifies it, the material is supplied against the European grade 1.4436 and the AFNOR designation is carried on the certificate. The table below is the recognised cross-reference set. As with all equivalence tables, the source standards should be checked for the specific application, because the ranges are close but not identical.
| Standard and region | Designation |
|---|---|
| France, AFNOR NF A 35-574 | Z7CND18-12-03, also Z7CND18-12-3 |
| Europe, EN 10088 | 1.4436 / X3CrNiMo17-13-3 |
| USA, AISI and UNS | 316 / S31600 |
| Japan, JIS | SUS316 |
| UK, BS | 316S33, 316S31 |
| Italy, UNI | X5CrNiMo17-13 |
| Sweden, SS | 2343 |
| China, GB | 0Cr17Ni12Mo2 |
| Poland, PN | H17N14M2 |
| Czechia, CSN | 17352 |
| Austria, ONORM | X5CrNiMo17-13-3KW |
| International, ISO | Type 20a |
Product standards that cover the grade
For forgings the two directly relevant European standards are EN 10222-5, steel forgings for pressure purposes in martensitic, austenitic and austenitic-ferritic stainless steels, and EN 10250-4, open-die steel forgings for general engineering purposes in stainless steels. The grade also appears in EN 10088-3 for bars and semi-finished products, EN 10272 for bars for pressure purposes, and EN 10028-7 for flat products.
Chemical composition
Two sets of limits are in circulation, and it pays to know which one your order is written against. The AFNOR standard NF A 35-574 is slightly wider on carbon and sulphur than the European specification for 1.4436. We can hold either set, and the applicable limits are stated on the order confirmation.
| Element | AFNOR min | AFNOR max | EN 1.4436 min | EN 1.4436 max |
|---|---|---|---|---|
| Carbon, C | – | 0.070 | – | 0.05 |
| Silicon, Si | – | 0.75 | – | 1.00 |
| Manganese, Mn | – | 2.00 | – | 2.00 |
| Phosphorus, P | – | 0.040 | – | 0.045 |
| Sulphur, S | – | 0.025 | – | 0.015 |
| Chromium, Cr | 16.50 | 18.50 | 16.50 | 18.50 |
| Nickel, Ni | 11.00 | 13.00 | 10.50 | 13.00 |
| Molybdenum, Mo | 2.50 | 3.00 | 2.50 | 3.00 |
| Nitrogen, N | – | not specified | – | 0.10 |
| Iron, Fe | Balance | |||
Check the specification before ordering. Z7CND18-12-03 is not a low carbon grade and carries no deliberate nitrogen addition. If the application needs the low carbon version for welded heavy sections, specify Z3CND18-12-03 / 1.4435 / 316L. If it needs nitrogen for higher strength, specify a 316LN type grade. Composition tables published for Z7CND18-12-03 that show C below 0.03 % together with N of 0.12 to 0.22 % are reproducing 316LN data and do not apply to this grade.
Mechanical and physical properties
Values apply to the solution annealed condition, tested in the longitudinal direction. Section size affects achieved properties in heavy forgings, so test piece location and sampling direction should be agreed at order stage for sections above roughly 160 mm.
| Property | Specification | Typical |
|---|---|---|
| 0.2 % proof strength, Rp0.2 | 200 N/mm2 min | 370 N/mm2 |
| Tensile strength, Rm | 500 to 700 N/mm2 | 670 N/mm2 |
| Elongation, A5 | 40 % min | 46 % |
| Hardness | 215 HB max | 200 HB |
| Impact energy, ISO-V at 25 °C | 100 J min | 220 J |
Proof strength at elevated temperature
| Temperature, °C | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 |
|---|---|---|---|---|---|---|---|---|---|---|
| Rp0.2 min | 175 | 158 | 145 | 135 | 127 | 120 | 115 | 112 | 110 | 108 |
Physical properties
| Property | Value |
|---|---|
| Density | 8.0 kg/dm3 |
| Modulus of elasticity | 200 GPa |
| Thermal conductivity | 15 W/m·K |
| Specific heat capacity | 500 J/kg·K |
| Electrical resistivity | 0.75 ohm·mm2/m |
| Coefficient of thermal expansion | 16.0 x 10-6 K-1 from 20 to 100 °C, rising to 18.0 x 10-6 K-1 from 20 to 500 °C |
| Magnetic behaviour | Non-magnetic in the annealed condition, relative permeability 1.3 or below |
| Service temperature | Suitable for use up to 700 °C, also suited to cryogenic applications |
Corrosion behaviour and its limits
Z7CND18-12-03 / 1.4436 is specified when the corrosion resistance of 1.4401 is no longer sufficient. Its pitting resistance equivalent of 24.75 to 30.16 sits slightly above 1.4401 because of the higher molybdenum, and the difference shows mainly in chloride containing environments. The grade performs well in most natural waters at moderate chloride and salt content, in food, beverage and agricultural service, and in a range of acid environments.
Two limits to design around. The grade is not resistant to sea water. For sea water duty, specify a super austenitic or super duplex grade such as A182 F44, A182 F55 or Alloy 31. Second, because of its relatively high carbon content it is not considered resistant to intergranular corrosion in the welded condition, although thin sections can be welded without that danger. Where welded heavy sections will see a corrosive medium, the low carbon 1.4435 / 316L route is the safer specification.
Welding
The grade is readily weldable by all common processes. Maximum interpass temperature is 150 °C and post-weld heat treatment is not normally required. Scale or heat tint from welding or high temperature processing must be removed mechanically or chemically, then passivated to restore the corrosion resistance.
Forging, heat treatment and machining
Hot working parameters
| Operation | Parameter |
|---|---|
| Pre-heat | 1150 to 1200 °C |
| Forging and rolling range | 1200 to 900 °C, finish above 900 °C |
| Cooling after forging | Rapid, in air or water, to avoid undesirable phases |
| Solution annealing | 1020 to 1120 °C, followed by rapid cooling in water or air |
| Hardening by heat treatment | Not possible. Austenitic grade, strengthened only by cold work |
One correction worth noting against older datasheets in circulation: the solution annealing window is 1020 to 1120 °C, not 1100 to 1150 °C.
Machining
Because of its higher alloy content, 1.4436 is more difficult to machine than 1.4401 or 1.4435. The figures below are the published starting point for coated carbide tooling on solution annealed material at Rm 560 to 640 N/mm2.
| Depth of cut | Feed | Cutting speed |
|---|---|---|
| 6 mm | 0.5 mm/rev | 115 m/min |
| 3 mm | 0.4 mm/rev | 145 m/min |
| 1 mm | 0.2 mm/rev | 185 m/min |
Z7CND18-12-03 forgings we produce
Every item below is forged from a single piece of steel melted on our own site. No castings, no welded fabrications, no purchased billet of unknown origin.
Seamless rolled rings
Rectangular and contoured sections ring-rolled from a punched preform, 50 mm to 6,000 mm outside diameter, for bearings, gears, flanges and pressure vessels.
Forged rings
Upset and punched rings for sections outside the ring mill envelope, plus gear rings, retaining rings and valve seat rings.
Forged flanges
Weld neck, blind, slip-on, socket weld, lap joint, orifice, anchor, girth, swivel and long weld neck to ASME B16.5, B16.47 and API 6A.
Forged shafts
Stepped, gear, pinion and eccentric shafts, spindles and rotors, quenched vertically in 15 m well type furnaces to control distortion.
Tube sheets and discs
Solid forged discs, tube sheets and covers for heat exchangers and pressure vessels, supplied proof-machined for volumetric inspection.
Valve and wellhead parts
Bodies, bonnets, blocks, stems, seat rings, spools, nozzles and manifolds for ball, gate, globe, check and plug valves.
Bars, blocks and billets
Round, flat and square bars and forged blocks as feedstock for machined bodies and tooling.
Cylinders, sleeves and pipes
Hollow forged cylinders, sleeves, bushings and heavy wall pipe sections bored from solid forged blanks.
Where the grade is used
Z7CND18-12-03 is applied where a 316 type stainless is wanted with more margin against chlorides and acids than 1.4401 gives, and where the service is not sea water. Published typical applications are the medical and pharmaceutical industries and the petrochemical industry, along with pumps, chemical storage tanks, pipework and installations, heat exchangers, coolers, and food, textile, paper and cryogenic equipment.
In forged form we supply it mainly as heat exchanger tube sheets, covers and shell flanges for chemical and pharmaceutical process plant, pump and valve bodies, bonnets, stems and seat rings, rolled rings and shafts for process machinery and agitators, and nozzles, sleeves and bushings for pressure vessels, columns and towers.
Sourcing Z7CND18-12-03 forgings from Jiangyin Jiangnan Metal
Most forging suppliers in China buy billet. Jiangyin Jiangnan Metal Co., Ltd. melts its own steel, which matters for a molybdenum bearing austenitic grade in two practical ways. The chemistry can be aimed at the forging it will become rather than accepted as delivered, and the certificate traces the part back to its melt number instead of stopping at a purchased billet certificate.
Stainless and duplex grades run through the 25 t electric arc furnace, are refined in 25 t and 50 t ladle furnaces and decarburised under vacuum in 30 t and 60 t VOD units, which is where carbon control is held. Maximum heat size is 60 tonnes. Steel then moves through the presses, the ring mill, 14 heat treatment furnaces and the machine shop without leaving the site.
| Product form | Size limit | Set by |
|---|---|---|
| Seamless rolled rings | 50 to 6,000 mm outside diameter | 6 m radial axial ring mill, plus 3 m and 1 m mills |
| Forged shafts | up to 14,000 mm turned length | C61160 horizontal lathe, 15 m well type furnace for vertical quench |
| Discs, tube sheets, blocks | up to 5,000 mm machined diameter | 5,000 mm swing vertical turning lathe |
| Bored cylinders, hollow shafts | up to 1,600 x 10,000 mm | CNC deep hole drilling machine |
| Single-piece weight | up to 30,000 kg | 60 t heat size, 6,300 t, 4,000 t and 2,000 t presses |
| Minimum order | 10 kg, no minimum piece count | Weight based, not quantity based |
| Lead time | 20 to 60 days | Standard stainless grades sit at the lower end |
Testing and certification
In-house testing. Melt analysis by optical emission spectrometry to ASTM E415, mechanical testing to ASTM A370 and ISO 6892 on 600 kN and 300 kN machines, Charpy V-notch impact with low temperature bath to minus 60 °C, ultrasonic testing to ASTM A388, EN 10228-3 or SEP 1921, magnetic particle to ASTM E709, PMI alloy verification, and metallography to ASTM E112 for grain size. Intergranular corrosion testing to ASTM A262, pitting tests to ASTM G48 and impact below minus 60 °C are placed with an accredited third party laboratory, so flag these at enquiry stage to have them scheduled before shipment.
Certification is EN 10204 3.1 as standard, or EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector on request. The works holds CCS, BV, DNV, LR and NK classification society approvals.
Frequently asked questions
What is Z7CND18-12-03 equivalent to?
It is the AFNOR designation for EN 1.4436 / X3CrNiMo17-13-3, an austenitic chromium-nickel-molybdenum stainless steel. It cross-references to AISI 316 (UNS S31600), JIS SUS316, BS 316S33 and 316S31, UNI X5CrNiMo17-13, SS 2343, GB 0Cr17Ni12Mo2, PN H17N14M2, CSN 17352 and ISO Type 20a.
Is Z7CND18-12-03 the same as 316L?
No. The Z7 prefix indicates about 0.07 % carbon. NF A 35-574 permits up to 0.070 % C and EN permits up to 0.05 % C for 1.4436, while 316L is a low carbon grade at 0.03 % maximum. The AFNOR low carbon counterpart is Z3CND18-12-03, which corresponds to 1.4435.
What are the mechanical properties in the solution annealed condition?
EN 10088-3 specifies Rm of 500 to 700 N/mm2, Rp0.2 of 200 N/mm2 minimum, A5 of 40 % minimum and hardness of 215 HB maximum, with ISO-V impact energy of 100 J minimum at 25 °C. Typical datasheet values are 370 N/mm2 proof strength, 670 N/mm2 tensile, 46 % elongation, 200 HB and 220 J.
At what temperature is Z7CND18-12-03 forged?
Pre-heat to 1150 to 1200 °C, forge between 1200 and 900 °C, then cool rapidly in air or water to avoid undesirable phases that would damage corrosion resistance and mechanical properties. Final solution anneal is 1020 to 1120 °C with rapid cooling.
Can it be used in sea water or in sour service?
Not sea water. With a pitting resistance equivalent of 24.75 to 30.16 it sits above 1.4401 but below the threshold for sea water service, so for that duty consider A182 F44, A182 F55, Alloy 31 or 904L. For sour service to NACE MR0175 and ISO 15156, state the requirement on the enquiry and we will advise on grade selection and hardness control.
What is the largest Z7CND18-12-03 ring you can roll?
6,000 mm outside diameter on the 6 m radial axial mill, with 3 m and 1 m mills for smaller sizes. The heaviest single forging in any grade is 30 tonnes, worked on 6,300 t, 4,000 t and 2,000 t hydraulic presses.
Is there a minimum order quantity?
10 kg, with no minimum piece count. The limit is weight, not quantity, so a single small part is quotable and so is a one-off large ring. Very small parts are grouped into a batch to share furnace and setup time, so quantity still affects unit price even though it does not affect whether we can take the job.
Can you supply finish machined parts, or rough forgings only?
Both. Forgings can be supplied as forged with machining allowance, proof-machined for ultrasonic testing, or finish machined to drawing. Heat treatment, machining, NDT and mechanical testing are all carried out in-house before shipment.
Request a quotation
Send these six items in the first email and we normally return a price within two working days. One, grade or specification, for example Z7CND18-12-03 or 1.4436. Two, dimensions or a drawing in PDF, DWG, DXF or STEP. Three, quantity and expected repeat volume. Four, delivery condition, as forged, proof-machined or finish machined. Five, heat treatment and testing requirements. Six, certification level and destination port.
Technical data compiled from AFNOR NF A 35-574, EN 10088-1 and EN 10088-3, and from published mill datasheets for EN 1.4436. Equivalence tables indicate the closest known equivalent grades only, so always check the source standard for your application. Last updated 11 October 2026.