Z2CNDU25-20 (904L / UNS N08904 / EN 1.4539) Forgings
Open-die forged rings, flanges, bars, shafts, discs, sleeves and tube sheets in super-austenitic stainless steel, made to drawing by Jiangyin Jiangnan Metal Co., Ltd.
Z2CNDU25-20 is the AFNOR designation for the super-austenitic stainless steel known internationally as 904L, UNS N08904 and EN 1.4539 (X1NiCrMoCu25-20-5). It is a low carbon grade, 0.02 percent C maximum, with high nickel and molybdenum content and 1 to 2 percent copper added for resistance to reducing acids, chiefly sulphuric acid. AFNOR documents also write the grade as Z2 NCDU 25-20. Both forms refer to the same material.
Jiangyin Jiangnan Metal Co., Ltd. is an open-die forging factory in Jiangyin, Jiangsu Province, China. We produce Z2CNDU25-20 forgings to customer drawings, including rolled rings, flanges, shafts, bars, discs, sleeves, bushings, hollow tubes and tube sheets, supplied solution annealed with EN 10204 3.1 or 3.2 certification.
Equivalent designations
| Standard | Designation |
|---|---|
| AFNOR, France | Z2 NCDU 25-20, also written Z2CNDU25-20 |
| Common trade name | 904L |
| ASTM / UNS | UNS N08904, forgings to ASTM A182 F904L |
| EN 10088 | 1.4539, X1NiCrMoCu25-20-5 |
| BS, UK | 904S13 |
| JIS, Japan | SUS 890L, SUS 317J5L |
| PN, Poland | 0H22N24M4TCu |
Compiled from published grade equivalence tables (Virgamet 1.4539 datasheet, Aircraft Materials 904L datasheet).
Chemical composition
Composition limits are not identical across standards. The AFNOR and EN versions are specified more tightly than the ASTM version, so a heat that meets UNS N08904 does not automatically meet Z2 NCDU 25-20. State the governing standard on the enquiry so the correct heat is selected.
| Element | ASTM UNS N08904 | AFNOR Z2 NCDU 25-20 | EN 1.4539 |
|---|---|---|---|
| C | 0.02 max | 0.02 max | 0.02 max |
| Cr | 19.0 to 23.0 | 19.0 to 21.0 | 19.0 to 21.0 |
| Ni | 23.0 to 28.0 | 24.0 to 26.0 | 24.0 to 26.0 |
| Mo | 4.0 to 5.0 | 4.0 to 5.0 | 4.0 to 5.0 |
| Cu | 1.0 to 2.0 | 1.0 to 2.0 | 1.2 to 2.0 |
| Mn | 2.0 max | 2.0 max | 2.0 max |
| Si | 1.0 max | 0.4 max | 0.7 max |
| P | 0.045 max | 0.035 max | 0.030 max |
| S | 0.035 max | 0.010 max | 0.010 max |
| N | 0.10 max | not specified | 0.15 max |
| Fe | Balance | ||
ASTM column from the AZoM grade 904L datasheet. AFNOR and EN columns from the Virgamet 1.4539 datasheet.
Mechanical properties
Values apply to the solution annealed condition. Acceptance values depend on product form and section size, so bar and forging requirements differ from plate requirements.
| Product and standard | Tensile strength | Yield, 0.2 percent proof | Elongation |
|---|---|---|---|
| Flat products, ASTM B625 | 490 MPa min | 220 MPa min | 36 percent min |
| Bars over 63 mm, EN 10088-5 | 530 to 730 MPa | 230 MPa min | 35 percent min |
| Bars 16 to 63 mm, EN 10088-5 | 530 to 880 MPa | 230 MPa min | 25 percent min |
ASTM B625 row from the AZoM grade 904L datasheet. EN 10088-5 rows as published in the Virgamet 1.4539 datasheet. The AZoM datasheet notes that its figures cover flat rolled products and may not apply to bar, tube and pipe.
Corrosion behaviour
The copper addition is what separates this grade from conventional 316L type steels. AZoM describes 904L as a non-stabilized austenitic stainless steel with copper added to improve resistance to strong reducing acids such as sulphuric acid, and as resistant to stress corrosion cracking and crevice corrosion. The grade is non-magnetic and offers good formability, toughness and weldability.
Resistance falls as acid concentration and temperature rise. Check corrosion data against the actual medium, concentration, temperature and chloride level before specifying.
PREN figures vary by source. Langley Alloys quotes a PREN of approximately 43 for a composition of around 20 percent chromium, 4 percent molybdenum and 1.5 percent copper. Other published figures for UNS N08904 are lower, because the result depends on the composition assumed and on whether a nitrogen term is included. For design work, calculate PREN from the heat analysis shown on the mill certificate rather than from a catalogue value.
904L compared with duplex and super duplex
Langley Alloys states that for most applications super duplex stainless steels match 904L on corrosion resistance while offering higher strength and lower cost, and that Ferralium 255 outperforms 904L in sulphuric acid because of its copper content. On their assessment the real advantage of 904L is its wider operating temperature range, holding up below minus 50 degrees Celsius or above 250 degrees Celsius where super duplex is limited. AZoM makes a similar point, noting that 904L contains high amounts of expensive molybdenum and nickel and that most applications using it today have been replaced by lower cost duplex 2205.
Where your duty falls inside the duplex temperature window, ask us to quote duplex alongside 904L. Getting the grade right costs less than replacing the part.
Forging and heat treatment
Suppliers of ASTM A182 F904L forgings cite a forging temperature range of 1000 to 1150 degrees Celsius. Solution annealing after forging is required, not optional, because it restores the corrosion resistance of the hot worked structure. AZoM gives 1090 to 1175 degrees Celsius followed by rapid cooling.
| Forging temperature | 1000 to 1150 degrees Celsius |
|---|---|
| Solution anneal | 1090 to 1175 degrees Celsius, rapid cooling |
| Hardening | Not hardenable by heat treatment, strengthened by cold work only |
| Welding | Readily welded. AZoM notes that subsequent annealing is not required in most cases, but should be carried out where fabrication is performed under severe stress corrosion cracking conditions |
| Machining | Standard methods. Low sulphur content gives a work hardening tendency, so use rigid setups and positive feed |
Forging range from ASTM A182 F904L flange supplier data (Ramesh Group). Annealing and welding guidance from the AZoM grade 904L datasheet.
Forged products in Z2CNDU25-20 / 904L
We produce this grade as open-die and ring-rolled forgings to customer drawings rather than from a stock catalogue. Usual shapes are seamless rolled rings and ring blanks, forged flanges and blind flanges, round bars and billets, straight and stepped shafts, discs, sleeves and bushings, hollow forged tubes and cylinders, tube sheets and nozzle forgings, valve bodies, bonnets, stems and seat rings, and pump casings and impeller blanks. General process capability is described on our open-die forged parts page.
Typical applications
AZoM lists the main applications of grade 904L as wiring in electrostatic precipitators, oil refinery components, seawater cooling devices, gas scrubbing plants, pulp and paper processing, and acetic, phosphoric and sulphuric acid processing plants. Forgings in this grade are normally specified for the pressure-retaining and rotating parts within that equipment.
Inspection and certification
Forgings are supplied with ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388 as agreed on order, together with chemical analysis, mechanical testing in the final heat treated condition and a dimensional report. Certificates are issued to EN 10204 3.1, or 3.2 with third party witness. Intergranular corrosion testing to ASTM A262 and PMI verification can be added. Confirm the test package at enquiry stage, since it affects lead time and price.
Frequently asked questions
Is Z2CNDU25-20 the same as 904L?
Yes. Z2CNDU25-20 (AFNOR), 904L, UNS N08904, EN 1.4539 and BS 904S13 name the same super-austenitic stainless steel. Composition limits differ between standards, with the AFNOR and EN versions specifying narrower chromium and nickel bands and tighter sulphur and silicon than ASTM UNS N08904. Quote the standard shown on your drawing.
Why is the grade written both Z2 NCDU 25-20 and Z2CNDU25-20?
AFNOR naming lists element letters in order of decreasing content. With around 25 percent nickel ahead of 20 percent chromium, the formal designation is Z2 NCDU 25-20. The form Z2CNDU25-20 is widely used in trading documents and refers to the same steel.
What sizes can you forge?
Capability depends on the shape and on mill availability of the grade, so we confirm it per enquiry. Send the outside diameter, inside diameter, height or length, quantity, and whether you need rough or finish machined condition.
What certification is issued?
EN 10204 3.1 as standard. EN 10204 3.2 with third party inspection on request, covering heat analysis, mechanical properties after solution annealing, NDT results and dimensional report.
What information is needed for a quotation?
A drawing or rough dimensions, the quantity, the governing standard (AFNOR Z2 NCDU 25-20, ASTM A182 F904L or EN 1.4539), and any NDT or certification requirements. Quotations are normally returned within one working day.
Request a quotation
Jiangyin Jiangnan Metal Co., Ltd., Open-Die Forging Factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel, WhatsApp and WeChat: +86 189-2135-9659
Email: sales@steelforgepieces.com
Page reviewed . Published by Jiangyin Jiangnan Metal Co., Ltd. Property data on this page is compiled from published standards and public datasheets and is given for guidance. It does not replace the mill certificate for a specific heat and is not a warranty of performance in service.