Jiangyin Jiangnan Metal Co., Ltd. — Open-Die Forging Factory No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China Tel: 0086-189-2135-9659 Email: sales@steelforgepieces.com
Jiangyin Jiangnan Metal Co., Ltd. Open-die forgings, rolled rings, forged flanges and shafts
High-alloy austenitic stainless · Open-die forgings

Z1NCDU31-27-03 Forgings — Alloy 28 / UNS N08028 / EN 1.4563

Z1NCDU31-27-03 is the French-style designation for the high-alloy austenitic stainless steel known internationally as Alloy 28, UNS N08028 and EN 1.4563 (X1NiCrMoCu31-27-4), sold by Alleima under the Sanicro 28 brand. It is a nickel-iron-chromium alloy with molybdenum and copper additions, nominally 31% Ni, 27% Cr, 3.5% Mo and 1% Cu, used in strong acids and chloride-bearing media.

Jiangyin Jiangnan Metal Co., Ltd. forges this grade to customer drawing as rolled rings, flanges, shafts, discs, sleeves, bushings, tube sheets and bars. Parts are solution annealed, ultrasonically tested to EN 10228-4 or ASTM A745, and released with EN 10204 3.1 or third-party 3.2 certification.

  • Z1NCDU31-27-03
  • Alloy 28
  • UNS N08028
  • EN 1.4563
  • X1NiCrMoCu31-27-4
  • Sanicro 28
  • NF Z2NCDU31-27
  • Nicrofer 3127 LC
  • GOST 02Ch27N31M4
  • Remanit 4563
Designation note: cross-reference tables list the NF designation for this alloy as Z2NCDU31-27. The spelling Z1NCDU31-27-03 is in common commercial use and is the form many buyers enquire with. If your drawing is written to a specific national standard, send us the exact callout and we will confirm the chemistry and acceptance criteria before quoting.

Summary data

Z1NCDU31-27-03 / Alloy 28 forgings supplied by Jiangyin Jiangnan Metal Co., Ltd.
Alloy familyHigh-alloy austenitic stainless steel, Ni-Fe-Cr-Mo-Cu
UNS numberN08028
EN material number1.4563, X1NiCrMoCu31-27-4
Reference standardsEN 10088-1, ISO 21457
Nominal composition31 Ni / 27 Cr / 3.5 Mo / 1 Cu, balance Fe
Density8.0 g/cm³ (0.289 lb/in³)
PRE numberMinimum 38, per Alleima data for Sanicro 28
Forging temperature1150-850 °C (2100-1560 °F)
Solution annealing1050-1150 °C (1920-2100 °F), rapid quench
Welding groupISO 8.2, preheating not required
Melting routeEAF + VOD, ESR remelt on request
CertificationEN 10204 3.1, or 3.2 countersigned by third party
SupplierJiangyin Jiangnan Metal Co., Ltd., Jiangyin, Jiangsu, China

Chemical composition

Two sets of limits exist for this grade and they are not the same. The ISO / UNS N08028 limits are the wider of the two. EN 1.4563 is tighter on carbon, silicon, sulphur and nickel, and caps nitrogen. State which one your order is written to, because a heat that passes N08028 will not automatically pass 1.4563.

Weight percent. ISO column per UNS N08028, EN column per EN 1.4563, NF column per Z2NCDU31-27.
ElementISO / UNS N08028EN 1.4563NF Z2NCDU31-27
Nickel (Ni)30.0-34.030.0-32.030.0-32.0
Chromium (Cr)26.0-28.026.0-28.026.0-28.0
Molybdenum (Mo)3.0-4.03.0-4.03.0-4.0
Copper (Cu)0.6-1.40.7-1.50.7-1.5
Carbon (C)0.030 max0.02 max0.02 max
Silicon (Si)1.00 max0.70 max0.50 max
Manganese (Mn)2.50 max2.00 max2.00 max
Phosphorus (P)0.030 max0.030 max0.025 max
Sulphur (S)0.030 max0.010 max0.010 max
Nitrogen (N)not specified0.10 maxnot specified
Iron (Fe)BalanceBalanceBalance

Mechanical properties, solution annealed

Values below apply to forgings in the hot-worked and solution-annealed condition (+AT) at 20 °C. Alloy 28 is single-phase austenitic and is not hardenable by heat treatment. Strength above these levels comes only from cold work, which rarely applies to heavy forgings.

Room-temperature properties of 1.4563 forgings, +AT condition. Actual values are confirmed per heat on the mill certificate.
PropertyMetricImperial
Proof strength Rp0.2≥ 220 MPa≥ 32 ksi
Tensile strength Rm500-700 MPa73-102 ksi
Elongation A≥ 40%≥ 40%
Hardness≤ 230 HB≤ 230 HB
Impact KV, longitudinal, +20 °C≥ 100 J≥ 74 ft·lb
Impact KV, transverse, +20 °C≥ 60 J≥ 44 ft·lb
Impact KV, transverse, −196 °C≥ 60 J≥ 44 ft·lb
Modulus of elasticity195 GPa28,300 ksi

Strength at elevated temperature

Minimum proof and tensile strength of 1.4563 forgings at temperature, solution-annealed condition.
TemperatureRp0.2 min, MPaRm min, MPa
50 °C209485
100 °C190460
150 °C175445
200 °C160430
250 °C155410
300 °C150400
350 °C145395
400 °C135—
450 °C125—
500 °C120—
550 °C115—

Physical properties

PropertyValue
Density at 20 °C8.0 g/cm³
Specific heat at 20 °C450 J/(kg·K)
Thermal conductivity at 20 °C12 W/(m·K)
Linear expansion, 20-100 °C15.8 × 10-6/K
Linear expansion, 20-300 °C16.5 × 10-6/K
Linear expansion, 20-500 °C17.3 × 10-6/K
Modulus at 100 °C190 GPa
Modulus at 200 °C182 GPa
Modulus at 300 °C174 GPa
Modulus at 400 °C166 GPa
Modulus at 500 °C158 GPa

Corrosion behaviour

Alloy 28 sits between the super-austenitic stainless steels and the nickel-base alloys on both cost and performance. What sets it apart is 27% chromium combined with a deliberate copper addition, which gives it good behaviour in reducing acids, sulphuric and phosphoric in particular, while the 3-4% molybdenum and 31% nickel handle chlorides.

Published material data describes the grade as resistant to sour gas, phosphoric, sulphuric and acetic acids, and vinyl chloride, with corrosion resistance rated better than UNS N08904 / 904L / 1.4539. It is resistant to intergranular corrosion in the as-delivered condition, which the low carbon ceiling makes possible, and it resists stress corrosion cracking well, including in hot chloride environments. Alleima gives Sanicro 28 a minimum PRE number of 38, which indicates high resistance to chloride pitting relative to standard austenitic grades. The alloy falls in welding group ISO 8.2 and needs no preheat.

Sour service: Alloy 28 is widely used in oil and gas production, and modified N08028 has been studied for sour environments with high salinity. The permissible combination of H₂S partial pressure, chloride content, temperature and elemental sulphur for any corrosion-resistant alloy is set by NACE MR0175 / ISO 15156-3. We do not publish a blanket sour-service rating. Send your service envelope and we will confirm compliance, supplementary testing and hardness limits in writing before accepting the order.

Forged products in this grade

Everything below is produced by open-die forging and ring rolling to the customer's drawing or dimensional sheet. We do not hold this grade as finished stock. Each order is forged from certified billet.

Product formTypical applicationNotes
Seamless rolled ringsHeat exchanger shells, vessel courses, valve bodiesRadial-axial rolled, grain flow follows the circumference
Forged flangesPressure vessels, piping, air receiversWeld-neck, blind, slip-on, special bores to drawing
Forged shafts and spindlesPumps, agitators, compressors, gearboxesUpset and drawn out, stepped shafts machined to print
Forged discs and disksBlind covers, blanks for machiningUpset from billet with controlled reduction ratio
Forged tube sheetsShell-and-tube heat exchangersDrilled and finish-machined on request
Forged bushings and sleevesSubsea and downhole assemblies, wear partsBored and trepanned to cut machining allowance
Forged round barsValve stems, fasteners, machining stockPeeled or rough-turned finish available
Forged pipes and hollowsCorrosive-service pipework, nozzlesTrepanned from solid or expanded from hollow
Valve componentsBall, gate, globe, check and plug valvesBodies, bonnets, seat rings, stems, blocks
Blocks, blanks, near-net shapesGeneral machined componentsSaw-cut to length

Industries served

Chemical and petrochemical processing. Sulphuric and phosphoric acid plant. Shell-and-tube heat exchangers, coolers, tanks, pumps, pipelines and pressure vessels. Offshore and subsea oil production equipment and wellheads. Seawater and chloride-bearing cooling water circuits. Pulp and paper bleaching plant. Pharmaceutical and biochemical process equipment. Published descriptions of the grade also cite cryogenic service, mining platform components, and aircraft structures, screws and valves.

How we forge and test it

Melting and billet

Billet is procured to EAF + VOD practice, which is what delivers the low carbon and sulphur ceilings this grade needs. ESR remelting is offered where the application calls for better cleanliness and less segregation, typically on thick-section and pressure-retaining parts. ESR is quoted as an option, not applied by default.

Forging

Worked between 1150 and 850 °C. Alloy 28 has a narrower hot-working window than carbon or low-alloy steel and work-hardens quickly, so we plan reheats rather than force reduction at the bottom of the range. Minimum forging reduction ratio is agreed with the customer; 3:1 or 4:1 is usual for pressure-retaining parts.

Solution annealing

Annealed at 1050-1150 °C and quenched rapidly, normally in water. This dissolves precipitated phases and restores the fully austenitic structure, which is what secures intergranular corrosion resistance in the delivered condition. Furnace charts are supplied with the certificate on request.

Testing

Because Alloy 28 is austenitic, its coarse grain structure scatters and attenuates ultrasound far more than ferritic steel does. The correct ultrasonic specifications are therefore EN 10228-4, which covers austenitic and austenitic-ferritic stainless steel forgings, or ASTM A745/A745M for austenitic steel forgings. EN 10228-3 and ASTM A388 are written for ferritic and martensitic steels. If we receive those on a purchase order for this grade we will raise a technical query before proceeding.

TestSpecificationApplied
Ultrasonic testingEN 10228-4 or ASTM A745/A745MStandard on pressure-retaining parts
Liquid penetrantEN ISO 3452 or ASTM E165On request
Chemical analysisSpectrographic, per heatEvery heat, reported on certificate
Tensile and impactEN ISO 6892-1, EN ISO 148-1Per heat-treatment batch
Intergranular corrosionASTM A262, practice as specifiedOn request
HardnessBrinellStandard, mandatory on sour-service orders
Material identificationPMI / XRFOn request

Certification

Forgings are released with an EN 10204 Type 3.1 inspection certificate issued by our works inspection department, which is independent of manufacturing. Where the contract calls for it we arrange Type 3.2, which carries the additional countersignature of an independent inspector or the purchaser's representative. Third-party witnessing by agencies such as TUV, BV, SGS or Lloyd's is organised against the purchase order.

Machining

This alloy is considerably harder to machine than 316/316L. It work-hardens fast and conducts heat poorly, so heat concentrates at the cutting edge. In practice that means a large cut in surface speed against a standard austenitic grade, while feed should be reduced only slightly. Light feeds let the tool skid across the work-hardened layer and make matters worse. Use rigid setups, sharp positive-rake coated carbide, generous through-tool coolant, and avoid dwelling or re-entering the same cut. We can supply forgings with extra machining allowance where the customer's shop is not set up for high-alloy work.

Frequently asked questions

What is Z1NCDU31-27-03 equivalent to?

It corresponds to Alloy 28, UNS N08028 and EN 1.4563 (X1NiCrMoCu31-27-4), brand name Sanicro 28. Other listed equivalents include GOST 02Ch27N31M4, Nicrofer 3127 LC, Remanit 4563 and Nirosta 4563. Cross-reference tables give the NF designation as Z2NCDU31-27.

Is it a stainless steel or a nickel alloy?

It is classed as a high-alloy austenitic stainless steel, and is sometimes described as a nickel-iron-chromium alloy because iron is the balance while nickel reaches 30-34%. Suppliers catalogue it under both headings, which is why this page sits in our stainless steel section alongside our nickel alloy forgings.

What heat treatment is used?

Solution annealing at 1050-1150 °C followed by a rapid quench, normally in water. The alloy is fully austenitic and cannot be hardened by heat treatment. The anneal exists to dissolve precipitates and secure corrosion resistance, not to raise strength.

How does Alloy 28 compare with 904L?

Published material data rates Alloy 28 / 1.4563 as having better corrosion resistance than UNS N08904 / 904L / 1.4539. The higher chromium and the copper addition are the main reasons, particularly in sulphuric and phosphoric acid service.

Which ultrasonic standard applies?

EN 10228-4 or ASTM A745/A745M, both written for austenitic forgings. EN 10228-3 and ASTM A388 cover ferritic and martensitic steels and should not be specified for this grade.

What sizes can you forge?

Capability depends on the product form and the billet available for the heat. Send the drawing, finished weight and quantity to sales@steelforgepieces.com and we will confirm feasibility, reduction ratio and lead time with the quotation.

Can you supply EN 10204 3.2 certification?

Yes. Type 3.1 is issued as standard by our independent works inspection department. Type 3.2 adds the countersignature of an independent inspector or the purchaser's representative and is arranged against the purchase order.

Do you supply machined parts or only black forgings?

Both. We supply as-forged and heat-treated blanks, rough-machined forgings with an agreed allowance, and finish-machined components to drawing. Given how demanding this alloy is to cut, many customers find it cheaper for us to carry out the rough machining.

Request a quotation

Send a drawing, a sketch, or the dimensions and quantity. We quote open-die forgings in Alloy 28 / UNS N08028 to customer specification, with melting route, NDT level and certification grade confirmed in writing before order acceptance.

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China

GradeWhy it is considered alongside Alloy 28
Alloy 31 / UNS N08031Higher-alloyed austenitic grade in the same family for more aggressive acid duty
Incoloy 825Ni-Fe-Cr with Mo and Cu, routinely compared for acid and sour service
Incoloy 926 / UNS N08926Super-austenitic alternative for seawater and chloride service
Hastelloy C-276Ni-Mo-Cr alloy for conditions beyond the range of austenitic stainless
Inconel 625Ni-Cr-Mo-Nb alloy for high temperature and severe corrosion
A286Precipitation-hardening austenitic grade where higher strength is needed

Published , last reviewed . Technical data is compiled from published datasheets for EN 1.4563 / UNS N08028 and is given for guidance. Properties for a specific order are confirmed on the heat certificate.