Heat-resisting austenitic grade

X8CrNi25-21 EN 1.4845 · AISI 310S · UNS S31008 — open-die forgings, rolled rings and bar

X8CrNi25-21 is the EN chemical designation of the austenitic heat-resisting stainless steel numbered EN 1.4845, a 24 to 26 percent chromium and 19 to 22 percent nickel grade listed in EN 10095. Its closest American equivalent is AISI 310S / UNS S31008; SEW 470 calls the same material number X12CrNi25-21. The high chromium content builds a slow-growing, adherent oxide scale, which is why the grade is a default choice for furnace internals, radiant tubes and heat-exchanger parts running in air to about 1050 C. It is not hardenable by heat treatment.

We melt this grade ourselves rather than buying billet, so the certificate traces a finished ring or shaft back to its melt number instead of stopping at a purchased bar.

Grade data sheet1.4845
EN name
X8CrNi25-21
EN number
1.4845
UNS
S31008
Type
Austenitic, heat resisting, non-hardenable
Cr / Ni
24.0–26.0 / 19.0–22.0 %
Density
7.8–7.9 g/cm³
Max in air
approx. 1050 C
Condition
Solution annealed (+AT)
Max ring
OD 6,000 mm
Max piece
30,000 kg
Min order
10 kg
Lead time
20–60 days
01

Designations and equivalents

Cross-reference for material number 1.4845. These are nearest equivalents for enquiry purposes, not drop-in substitutions. Where a drawing names one standard, order against that standard.

Equivalent designations for 1.4845
Standard or regionDesignation
EN, chemical nameX8CrNi25-21
EN and SEW, material number1.4845 (also written 4845)
SEW 470X12CrNi25-21
ASTM / AISI / UNS310S, UNS S31008; also 310H, UNS S31009, TP310S
JIS, JapanSUS 310S
GB, China06Cr25Ni20 (0Cr25Ni20)
AFNOR, FranceZ12CN25-20
BS, United Kingdom310S24
GOST, Russia20Kh23N18, 10Kh23N18
PN, PolandH23N18
Related, not equivalentX16CrNi25-20 / 1.4843
02

Chemical composition

Weight percent. Single figures are maxima. The EN and ASTM limits differ on three elements, which is the most common source of rejected certificates on this grade.

EN 1.4845 compared with AISI 310S
ElementEN 1.4845 / X8CrNi25-21AISI 310S / UNS S31008
Carbon, Cmax 0.10max 0.08
Manganese, Mnmax 2.00max 2.00
Silicon, Simax 1.50max 1.50
Phosphorus, Pmax 0.045max 0.045
Sulphur, Smax 0.015max 0.030
Chromium, Cr24.00–26.0024.00–26.00
Nickel, Ni19.00–22.0019.00–22.00
Nitrogen, Nmax 0.11not specified
Iron, Febalancebalance
Ordering note The EN sulphur ceiling of 0.015 percent is half the ASTM ceiling, while the EN carbon ceiling of 0.10 percent is above the ASTM figure of 0.08 percent. A heat that passes 310S will not necessarily pass 1.4845 on sulphur, and a heat that passes 1.4845 will not necessarily pass 310S on carbon. If the order needs dual certification, say so at enquiry stage so the melt is aimed at the tighter of the two limits on every element.
03

Mechanical and physical properties

Room temperature values in the solution annealed condition. Acceptance criteria should always be read from the current edition of the governing standard; the figures here are for design orientation and enquiry.

Room temperature mechanical properties
PropertyEN 1.4845, typical or specifiedASTM A182 F310 forgings
Tensile strength, Rm500–700 MPa515 MPa min
Yield strength, Rp0.2min 210 MPa205 MPa min
Elongation, Amin 33 %per standard edition
Hardnessmax 192 HB, approx. 170 HB typical217 HB max
Modulus of elasticity, E196–200 GPa—
Shear modulus78 GPa—
Poisson's ratio0.27—
Physical and thermal data
PropertyValuePropertyValue
Density7.8–7.9 g/cm³Thermal conductivityapprox. 15 W/m·K
Specific heat, 20–100 C480–500 J/kg·KExpansion coefficient15–16 x 10⁻⁶ /K
Melting rangeapprox. 1360–1400 CLatent heat of fusion310 J/g
04

Creep limit and creep rupture strength

Values in MPa. These govern the sizing of any X8CrNi25-21 forging that carries load at temperature, and they fall away steeply above 700 C, which is the part designers most often miss when substituting this grade for a lower-alloy austenitic.

Creep data for 1.4845, MPa
Property600 C700 C800 C900 C
Creep limit R 1/1000100451810
Creep limit R 1/100009030104
Rupture strength Rz/1000170803515
Rupture strength Rz/1000013040188.5
Rupture strength Rz/100000801873
05

Forging and heat treatment

Hot working

Forging and ring rolling run between 1150 C and 950 C. Finishing below the lower limit risks cracking in a fully austenitic structure that work hardens as it cools. Plate elements are hot bent at 900 to 950 C.

Solution annealing

1100 to 1150 C, water quenched. This is the only standard treatment. The grade takes no benefit from quench and temper or from ageing, and strength comes from the alloy content rather than from any precipitation reaction.

Service temperature

Rated to roughly 1050 C in air and oxidising atmospheres. In reducing gases carrying higher sulphur concentrations the limit drops to about 900 C; where sulphur is only a minor impurity, about 1000 C is workable.

Sigma phase caution

As with other high-chromium austenitics, long exposure in the band around 650 to 900 C can precipitate sigma phase and cost room-temperature toughness. This matters for parts that cycle through that range rather than sitting above it.

Specification check Drawings for this grade occasionally arrive calling for solution treatment followed by ageing. X8CrNi25-21 is not an age-hardening alloy and no ageing step will raise its strength. Where a drawing carries that instruction we raise it before cutting steel, because the usual cause is a specification copied across from a precipitation-hardening grade such as A286 or 17-4 PH.
06

Product forms we forge in this grade

Everything is open-die forged or ring rolled to your drawing or size list. There is no stock catalogue and no minimum piece count; the minimum order is 10 kg.

X8CrNi25-21 forged product forms and applications
Product formTypical application
Seamless rolled rings, forged rings, retaining ringsKilns, furnace carriers and bases, radiant tubes, muffles, retorts, annealing covers
Forged flanges, tube sheets, nozzles, forged pipe sectionsPressure vessels, air receivers, shell and tube heat exchangers, preheaters
Forged shafts, spindles, eccentric shafts, round barGearboxes, gas compressors, turbine auxiliaries, power transmission
Forged discs, blanks, rolls, sleeves, bushingsSaggers, furnace fittings, conveyor rollers, oven linings, fan hubs
Valve bodies, bonnets, stems, seat rings, blocksBall, gate, globe, check and plug valves in hot service
Forged blocks, wheels, manifolds, machined to printProcess modules, chemical plant for gas pyrolysis, hydrogenation and methane conversion

Size envelope

Working limits set by plant equipment
ItemLimitSet by
Seamless rolled ringsOD 50 to 6,000 mm6 m radial-axial ring mill; upset and punch route below mill range
Shafts, turned lengthup to 14,000 mmC61160 horizontal lathe; 15 m well furnace for vertical quench
Discs, tube sheets, blocksup to 5,000 mm machined dia5,000 mm vertical turning lathe
Bored cylinders, hollow shafts1,600 mm dia x 10,000 mmCNC deep-hole drilling machine
Single piece weightup to 30,000 kg60 t maximum heat; 6,300 t press
07

Melting, testing and certification

X8CrNi25-21 runs through the electric arc furnace, is refined in the ladle furnace and is decarburised under vacuum, which is the route that holds the EN sulphur and nitrogen limits. Electroslag remelting is available where cleanliness or segregation control matters on heavy sections. Nothing in the melting, forging, heat treatment or machining sequence leaves the site.

Inspection and documentation
ItemScope
Melting routeEF plus LF plus VOD standard; ESR on request for heavy or critical sections
Ultrasonic testingEN 10228-3, SEP 1921 or ASTM A388, to the acceptance class you nominate
Surface examinationLiquid penetrant to ASTM E165 where specified
Mechanical testingRoom temperature tensile and hardness as standard; elevated temperature tensile on request
Corrosion testingIntergranular corrosion testing on request
CertificationEN 10204 3.1, or 3.2 with third party inspection
Approvals heldCCS, BV, DNV, LR, NK
AdditionalGrain size determination, PMI, melt number traceability to finished part
08

Common questions

Is X8CrNi25-21 the same thing as 310S?

Equivalent, not identical. Both are 25Cr-20Ni austenitics sharing the same chromium and nickel bands, but EN 1.4845 allows C max 0.10, S max 0.015 and N max 0.11, while AISI 310S allows C max 0.08 and S max 0.030 with no nitrogen limit. State which standard governs the order.

What is the difference between 1.4845 and 1.4843?

1.4843, X16CrNi25-20, is a different grade: carbon to 0.20 percent, a lower chromium band of 22.0 to 25.0 percent, and silicon deliberately raised to 1.5 to 2.5 percent. It is not an automatic substitute.

Can you certify to ASTM A182 F310 rather than EN?

Yes. Forgings can be ordered against EN 10095 practice or against ASTM A182 F310 and ASTM A473 for general stainless forgings. Give us the governing specification, the NDT class and the certificate type with the enquiry.

Do you have a minimum order quantity?

10 kg, with no minimum piece count. Single prototype forgings are accepted. Normal lead time runs 20 to 60 days depending on section size, heat treatment and machining scope.

How is X8CrNi25-21 welded?

Normally arc welded with matching high-alloy consumables; the established practice for the equivalent H23N18 grade uses ES-24-18 type electrodes. Procedure qualification should reflect the service temperature the component will actually see.

Do you buy billet or melt your own steel?

We melt. Most forging suppliers in China buy billet and the certificate chain stops at the purchase. Here the chemistry is aimed at the forging it will become, and the certificate traces back to the melt number.

09

Request a quotation

Send the drawing or the size list. A quotation comes back with price, forging route and delivery. Quotes move fastest when the enquiry states the grade and governing standard, finished or rough dimensions, quantity, heat treatment condition, NDT requirement and certificate type.

Jiangyin Jiangnan Metal Co., Ltd.

Integrated melting works, open-die forge and ring rolling mill. Operating since 1997, 460 staff, CCS, BV, DNV, LR and NK approved.

Plant  No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone  +86 189 2135 9659
Email  sales@steelforgepieces.com
Web  www.steelforgepieces.com

Email the drawing

10

Related grades

Grades specified alongside X8CrNi25-21 where service temperature, carburisation resistance or corrosion duty shifts the selection.

Reference standards

EN 10095 heat resisting steels and nickel alloys · EN 10088-1 list of stainless steels · SEW 470 · ASTM A182 / A182M grade F310 · ASTM A473 stainless steel forgings · EN 10228-3 and ASTM A388 ultrasonic examination of forgings · SEP 1921 · EN 10204 inspection documents.

Page maintained by the engineering office, Jiangyin Jiangnan Metal Co., Ltd., Jiangyin, Jiangsu, China.
Last reviewed . Composition and creep figures are taken from published EN 10095 and SEW 470 grade listings; forging product data reflects this plant's equipment. Verify all values against the current edition of the applicable standard before design release.