GRADE X7CrNiNb18-10  /  W.-NR. 1.4912  /  UNS S34709 MELTED AND FORGED IN ONE WORKS · JIANGYIN, CHINA · SINCE 1997 +86 189 2135 9659 · sales@steelforgepieces.com
Jiangnan Metal Open-Die Forging & Ring Rolling Request a quotation

Stainless steel grade datasheet

X7CrNiNb18-10 · 1.4912 Niobium-stabilised austenitic creep-resisting steel. Forged rings, flanges, bars, discs and shafts to drawing.

X7CrNiNb18-10 is the EN name for material number 1.4912, the creep-resisting member of the niobium-stabilised 18-10 family and the European counterpart of AISI 347H / UNS S34709. Jiangyin Jiangnan Metal melts this grade in its own furnaces and forges it on a 6,300 t press and a 6 m ring mill, from 10 kg test pieces up to 30 t single forgings.

Grade recordEN 10088-1
EN name
X7CrNiNb18-10
Material no.
1.4912
Group
Austenitic creep-resisting steel
USA
AISI 347H · UNS S34709
Japan
SUS347H
France
Z8CNNb18-10
Density
7.9 g/cm³
Condition
+AT, solution annealed
01

What the grade is, and what it is not

X7CrNiNb18-10 appears in the European stainless steel list EN 10088-1 and in EN 10216-5 for seamless tubes for pressure purposes, where it sits in the austenitic creep-resisting group rather than among the plain corrosion-resisting austenitics. The Applus+ material record states its purpose plainly: the corrosion resistant steel X7CrNiNb18-10 (1.4912) is used in pressure vessel engineering. For forgings the governing European document is EN 10222-5, steel forgings for pressure purposes, part 5, martensitic, austenitic and austenitic-ferritic stainless steels.

1.4912 is not 1.4550. Two niobium-stabilised 18-10 grades sit beside each other in the EN system and enquiries mix them up constantly. X7CrNiNb18-10 (1.4912) is the higher-carbon creep-resisting grade matching 347H. X6CrNiNb18-10 (1.4550) is the ordinary corrosion-service grade matching AISI 347, and EN 10216-5 lists it as a separate entry with its own tensile range and a mandatory intergranular corrosion test. If the design relies on strength above roughly 540 °C, state 1.4912 on the order.

The niobium is the point of the alloy. It raises yield strength at elevated temperature, and it ties up carbon as niobium carbide in preference to chromium carbide, so chromium stays in solution and the steel resists intergranular attack after time spent in the sensitising range. That is why stabilised grades are chosen for welded and thermally cycled pressure parts instead of plain 304 or 304L.

02

Chemical composition

X7CrNiNb18-10 / 1.4912, percentage by weight
LimitCSiMnPSCrNiNbFe
Min0.04––––17.09.00.40Balance,
approx. 64.6 to 73.6
Max0.101.002.000.0450.01519.012.01.20

Elements not listed are not added intentionally without agreement at the order stage. Niobium content is conventionally tied to carbon content for stabilisation; the window above is the standardised range for 1.4912.

03

Mechanical properties

Specified minima, EN 10216-5

Ambient temperature requirements, with 1.4550 shown for comparison
PropertyX7CrNiNb18-10 · 1.4912X6CrNiNb18-10 · 1.4550
Proof strength Rp0.2, min205 MPa205 MPa
Proof strength Rp1.0, min240 MPa240 MPa
Tensile strength Rm510 to 710 MPa510 to 740 MPa
Elongation A, min, longitudinal40 %35 %
Elongation A, min, transverse30 %30 %
Intergranular corrosion testNot required (creep-resisting group)Required

Condensed from the BSSA summary of EN 10216-5. The full standard governs in case of doubt.

Typical values, solution annealed

Indicative properties in the +AT condition
PropertyValuePropertyValue
Tensile strength, ultimate610 MPaBrinell hardness180 HB
Yield strength, proof230 MPaCharpy V-notch impact90 J
Elongation at break40 %Fatigue strength200 MPa
Young's modulus200 GPaShear modulus77 GPa
Shear strength420 MPaPoisson's ratio0.28

Physical and thermal data

Guideline figures for design checking
PropertyValuePropertyValue
Density7.8 to 7.9 g/cm³Thermal conductivity16 W/m·K
Melting onset, solidus1390 °CSpecific heat capacity480 J/kg·K
Melting completion, liquidus1430 °CThermal expansion16 µm/m·K
Maximum temperature, mechanical940 °CLatent heat of fusion290 J/g
Maximum temperature, corrosion520 °CModulus of elasticity200 GPa

Density is quoted as 7.9 g/cm³ by the European steel number database and 7.8 g/cm³ by makeitfrom; both are normal for an 18-10 austenitic. Temperature limits are orientation values only and must be checked against the design code in force for the equipment.

04

Equivalents and cross-reference

Closest known equivalents to X7CrNiNb18-10
Region or systemDesignationWhere it appears
Europe, ENX7CrNiNb18-10 · 1.4912EN 10088-1, EN 10216-5, EN 10222-5
United States, UNSS34709ASTM A959
United States, AISIType 347HAISI designation system
Japan, JISSUS347HJIS designation system
France, AFNORZ8CNNb18-10AFNOR designation system

Cross-reference tables indicate the closest known equivalents only. Source standards should always be checked for the specific purpose of each material.

05

How we make it

Most forging suppliers in China buy billet. This works starts one step earlier, at the furnace, so the chemistry can be aimed at the forging it will become and the certificate traces the part back to its melt number.

Melting

Stainless grades including 1.4912 run through the electric arc furnace, are refined in the ladle furnace and are decarburised under vacuum where carbon and nitrogen have to be held tight. Maximum heat size is 60 t. Where a customer specification calls for a remelted product, the protective-atmosphere electroslag route is available on site.

Forging and ring rolling

Heavy cogging and upsetting run on the 6,300 t press, with 4,000 t and 2,000 t presses and a bank of hammers for smaller work. Rings are rolled on radial-axial mills of 6 m, 3 m and 1 m, which covers outside diameters from about 50 mm on the upset-and-punch route up to 6,000 mm rolled. Heaviest single piece is 30 t.

Heat treatment

The delivery condition for this grade is +AT, solution annealed and water quenched. Quench annealing of an austenitic stainless steel is a rapid water cool whose purpose is to overcome sensitisation, so cooling rate through the carbide precipitation range matters more than the soak itself. 1.4912 is not precipitation hardening and cannot be aged, so any specification asking for solution plus age on this grade is queried before production starts. Fourteen furnaces are on site, including car-bottom chambers up to 8,000 mm long and 15 m deep well furnaces for vertical quenching of long shafts.

Machining

Stabilised 18-10 austenitics work-harden fast. Rigid set-ups, sharp positive-rake tooling, a heavy uninterrupted feed that stays under the hardened layer and generous coolant are what make the difference. Proof machining on the vertical lathes, up to 5,000 mm swing, is normal before volumetric inspection on discs and tube sheets.

Inspection and certification

Ultrasonic examination to EN 10228-3, SEP 1921 or ASTM A388 as agreed. Certification to EN 10204 3.1, or 3.2 countersigned by a third party. The works holds CCS, BV, DNV, LR and NK approvals. Chemical analysis, tensile and impact testing, intergranular corrosion testing, grain size, PMI and a dimensional report can all be built into the documentation package.

06

Product forms in X7CrNiNb18-10

Seamless rolled rings

Rectangular or contoured section, rolled from a punched preform, up to 6,000 mm outside diameter.

Forged rings

Upset and punched rings for sections outside the mill envelope, including seat rings and retaining rings.

Flanges

Weld neck, blind, slip-on, long weld neck, orifice and spectacle blinds, plus non-standard flange blanks.

Bars and blocks

Round, flat and square bar, black, turned or peeled, cut to the lengths on the order.

Discs and tube sheets

Solid forged discs, covers and tube sheets for exchangers and vessels, supplied proof machined.

Shafts and spindles

Stepped shafts, pinion shafts and eccentric shafts, up to 14,000 mm turned length.

Sleeves and bushings

Hollow forgings bored from solid, up to 1,600 mm diameter by 10,000 mm on the deep-hole drill.

Valve components

Bodies, bonnets, blocks, stems and seat rings for ball, gate, globe, check and plug valves.

07

Where the grade is used

Because 1.4912 belongs to the creep-resisting group and is written into standards for pressure tubing and pressure vessel work, its forged counterparts go where elevated-temperature strength and stabilised corrosion behaviour are both needed. That means refinery and petrochemical process plant, including catalytic cracking and reformer service; boiler and superheater headers; shell and tube heat exchangers, columns, towers and process modules; waste heat recovery and recuperators; power generation; and the flange, valve and nozzle packages that connect all of it. Offshore and compressor hardware uses the same grade where the duty is hot rather than chloride-driven. The 520 °C corrosion figure and the 940 °C mechanical figure quoted above are orientation values; the controlling design code always takes precedence.

08

Questions we get asked

What is X7CrNiNb18-10?

The EN chemical designation for material number 1.4912, a niobium-stabilised austenitic creep-resisting chromium-nickel stainless steel used in pressure vessel engineering and in seamless pressure tubing to EN 10216-5. Density 7.9 g/cm³, normally delivered solution annealed.

What is X7CrNiNb18-10 equivalent to?

AISI 347H and UNS S34709 in the United States, listed under ASTM A959; SUS347H in Japan; Z8CNNb18-10 in France.

Is X7CrNiNb18-10 the same as 1.4550?

No. 1.4912 is X7CrNiNb18-10, the creep-resisting grade matching 347H. 1.4550 is X6CrNiNb18-10, matching standard AISI 347. EN 10216-5 lists them separately with different tensile ranges and different intergranular corrosion test requirements.

Can the grade be hardened by heat treatment?

No. It is single phase austenitic, so it cannot be aged or quench hardened. Strength above the annealed minima comes only from cold work, and cold work builds quickly because the grade work-hardens fast. The specified treatment is solution annealing followed by a rapid water cool.

Why is transverse elongation lower than longitudinal?

Forged and tubular products have directional grain flow, so ductility measured across the flow is lower than along it, and EN 10216-5 sets separate minima for the two directions. Tell us which direction your end user will test in, so the forging route and the test piece location are planned from the start rather than argued about at inspection.

What sizes and quantities do you take?

Parts are forged to drawing rather than sold from a catalogue. Single pieces run from 10 kg to 30 t, with no minimum piece count, and normal lead time is 20 to 60 days depending on size, heat treatment and testing. Send the drawing or the rough dimensions together with the governing standard, delivery condition, NDT acceptance class and certificate type, and the quotation will come back with weight, tolerance, price and date.

09

References

  1. Applus+ Laboratories materials portal, X7CrNiNb18-10 / 1.4912 datasheet: standard scope, pressure vessel remark, UNS and AISI cross-reference.
  2. makeitfrom.com, EN 1.4912 (X7CrNiNb18-10) stainless steel: composition ranges, typical mechanical, thermal and physical values, role of niobium.
  3. British Stainless Steel Association, ambient temperature mechanical properties for EN 10216-5: specified proof and tensile strengths for 1.4912 and 1.4550.
  4. steelnumber.com, X7CrNiNb18-10 / 1.4912 and 347H worldwide equivalents: classification as austenitic creep-resisting steel, density, equivalence to 347H, S34709, SUS347H and Z8CNNb18-10.
  5. AZoM, stainless steel heat treatment: quench annealing as rapid water cooling to overcome sensitisation.

Data on this page is given for guidance. The governing standard and the design code for your equipment take precedence in all cases.