X2CrNiMo18-14-3 (EN 1.4435 / AISI 316L / UNS S31603) Open-Die Forgings

X2CrNiMo18-14-3 is the EN designation of stainless steel number 1.4435. It is a low-carbon austenitic CrNiMo steel with 17.0 to 19.0 % Cr, 12.5 to 15.0 % Ni and 2.50 to 3.00 % Mo, carbon limited to 0.030 %. The analysis sits inside the UNS S31603 (316L) window but at the richer end of it, which is why the grade is usually called the high-alloyed or acid-resistant 316L. Jiangyin Jiangnan Metal Co., Ltd. forges it to drawing as rings, seamless rolled rings, flanges, bars, discs, shafts, sleeves and tube sheets, delivered solution annealed with EN 10204 3.1 or 3.2 certification.

Grade at a Glance

Identification data for X2CrNiMo18-14-3 / 1.4435
EN name and numberX2CrNiMo18-14-3, 1.4435
AISI / UNS316L / S31603
StructureAustenitic, low ferrite after solution annealing
PREN, Cr + 3.3Mo + 16N25.3 to 30.7, calculated from EN composition limits
Hot forming range1150 to 850 °C, air cooling
Solution annealing1030 to 1110 °C, water or air cooling
Typical hardness215 HB max, solution annealed
Melting practiceEAF + VOD, ESR on request
Delivery conditionSolution annealed, pickled or machined

Chemical Composition

Heat analysis in %, maximum values unless a range is given, EN 10088 series
CSiMnPSNCrMoNiFe
0.0301.002.000.0450.0150.10 17.00 to 19.002.50 to 3.0012.50 to 15.00Balance

A controlled sulphur content of 0.015 to 0.030 % is permitted where machinability matters. EN 10088-3 for bars, rods and sections allows S up to 0.030 %, while flat product practice and most mill data sheets hold it at 0.015 %. For PREN ranking the BSSA uses N 0.11 % max. The restricted BN2 analysis can be specified for pharmaceutical work.

Mechanical Properties, Solution Annealed

EN 10088-3 minimum values for long products in the solution annealed condition
Thickness or diameterRp0.2 MPa minRp1.0 MPa minRm MPaElongation A % minHardness HB
up to 160 mm200235500 to 70040215 max
over 160 up to 250 mm200235500 to 70030215 max

Impact energy, ISO-V, room temperature, section 10 mm and above, is commonly quoted at 100 J minimum longitudinal. Hardness is for guidance only. For rods only the tensile strength values apply. Elevated temperature proof strength for pressure design is given in EN 10222-5 and AD 2000 W2 and W10; ask us for the table covering your section size.

Physical Properties

Room temperature data
Density at 20 °C8.0 kg/dm³
Modulus of elasticity at 20 °C200 kN/mm²
Modulus at 200 / 400 / 500 °C186 / 172 / 165 kN/mm²
Thermal conductivity at 20 °C15 W/(m·K)
Specific heat at 20 °C500 J/(kg·K)
Electrical resistivity at 20 °C0.75 Ω·mm²/m
Mean coefficient of linear expansion, 10-6 K-1, from 20 °C
to 100 °C200 °C300 °C400 °C500 °C
16.016.517.017.518.0

Austenitic steels conduct heat at roughly 30 % of the rate of unalloyed steel and expand considerably more, so distortion has to be controlled in both forging and welding.

International Equivalents

Designations cross-referenced to X2CrNiMo18-14-3 / 1.4435
Region or standardDesignation
EN, GermanyX2CrNiMo18-14-3, 1.4435
USA, AISI and UNS316L, S31603
USA, ASTM forgingsA182 F316L, A965 grade F316L
Japan, JISSUS316L, forgings SUSF316L to JIS G 3214
France, AFNORZ3CND18-14-03
United Kingdom, BS316S13
Sweden, SS2353
Russia, GOST03Ch17N14M3, forgings 03Ch17N14M2
South Korea, KSSTSF316L to KS D 4115
ISOX2CrNiMo17-3 to ISO 9327-5

Cross-references are approximate. Composition ranges, testing and delivery conditions differ between standards, so equivalent grades are not always interchangeable. We work to the standard named in the order.

Standards for Forged Products

European

EN 10222-5 covers stainless austenitic steel forgings for pressure purposes and lists 1.4435 for service from -10 to 400 °C. EN 10250-4 covers open die forgings in stainless steel for general engineering. EN 10088-3 covers semi-finished products, bars, rods and sections. EN 10272 covers bars for pressure purposes. AD 2000 W2 and W10 apply to pressure vessel use.

American and other

ASTM A182 and ASME SA182 for forged flanges and fittings, ASTM A965 grade F316L for forged or rolled parts in high temperature service, ASTM A276 and ASTM A479 or SA479 for bars and shapes. Supplier listings also cite 1.4435 against NACE MR0175 and ISO 15156-3 and the Pressure Equipment Directive. Confirm the specific requirement with us before ordering.

Forging and Heat Treatment

X2CrNiMo18-14-3 is hot formed between 1150 and 850 °C and cooled in air. Solution annealing follows at 1030 to 1110 °C with rapid cooling in water or air, which gives an austenitic structure with a low ferrite content. Where a continuous annealing furnace is used the upper part of that range is normally preferred. Where annealing takes place during further processing, aim at the lower part, otherwise the mechanical properties can be affected. Solution annealing may be omitted if hot forming and the cooling that follows already deliver the required mechanical properties and the intergranular corrosion resistance set out in EN ISO 3651-2.

After quenching the material can be slightly magnetisable, and magnetisability rises with cold forming. This is worth noting if your inspection plan includes a magnetic permeability check.

Corrosion Behaviour

Carbon capped at 0.030 % secures resistance to intergranular corrosion both as supplied and in the welded condition, verifiable to ASTM A262 practice E or EN ISO 3651-2. Molybdenum of 2.50 to 3.00 % raises resistance to pitting and crevice attack in chloride-bearing media. The calculated PREN range of 25.3 to 30.7 puts 1.4435 above the 23.1 to 28.5 band of 1.4401 and 1.4404, below 904L at 32.2 to 39.9, and well below 1.4547 at 42.2 to 47.6. PREN is a ranking tool only and does not prove a grade is suitable for a given duty. For hot chlorides or sour service, send the process conditions and we will discuss whether a duplex or super-austenitic forging is the safer choice.

Forgings We Manufacture in This Grade

Open-die and rolled-ring product forms in 1.4435 / 316L
Product formTypical use
Forged rings and seamless rolled ringsVessel shell courses, valve bodies, pump casings, bearing and gear blanks
Forged flanges, weld neck, slip on, blind and specialChemical and petrochemical piping, heat exchangers, pressure vessels
Forged round bars and shaftsPump and agitator shafts, valve stems, spindles, fasteners
Forged discs, blanks and tube sheetsHeat exchangers, closures, blind covers, gear and wheel blanks
Forged sleeves, bushings and hollow barsSubsea and offshore equipment, compressors, bearings
Forged pipes, nozzles and tubesReactor nozzles, piping transitions, pressure-retaining components
Forged valve partsBodies, bonnets, seat rings and blocks for ball, gate, globe, check and plug valves

All items are made to order. State outside diameter, wall, height or length, finished weight and quantity in your enquiry and we will confirm the forging envelope and the machining allowance.

Where This Grade Is Used

Common fields are chemical and petrochemical processing, petroleum refining, pharmaceutical and medical equipment, food and beverage production and storage, synthetic fibre, textile and artificial silk plants, pulp and paper equipment, semiconductor and electronic equipment manufacture, offshore modules, chemical tanks and pipework, and pressure vessels in general. In bioprocessing, 316L in the form of 1.4404 or 1.4435 is the most widely used material worldwide, with 1.4435 chosen where the higher Cr, Mo and Ni margin and the lower weld ferrite are wanted.

Welding

TIG, MAG solid wire, manual arc, submerged arc and laser beam welding are all usable, and the grade is rated weldability class A for laser beam welding under DVS 3203 part 3. Matching 316L filler such as Thermanit GE-316L (1.4430) is standard, with higher-alloyed fillers such as 1.4576 or 1.4440 where corrosion loading or the cast structure of the weld metal calls for it. Preheat is not required and post-weld heat treatment is not normally applied. Because thermal conductivity is low and expansion high, use lower heat input and higher travel speed than for unalloyed steel, prefer stringer beads, keep tack welds close together, and use a double-V preparation above 12 mm. Only stainless tooling and brushes should touch the surface. Annealing colours, scale, slag and tramp iron must be removed by brushing, grinding, pickling or iron-free blasting so the passive layer can re-form.

Testing, Inspection and Certification

Forgings in this grade can be supplied with chemical analysis, mechanical testing, ultrasonic examination to EN 10228-3, SEP 1921 or ASTM A388, intergranular corrosion testing to ASTM A262 practice E or EN ISO 3651-2, ferrite measurement, PMI, dimensional report and heat treatment charts. Certification is issued as EN 10204 3.1, or 3.2 countersigned by a third party such as TUV, BV, DNV, LR or SGS where the project calls for it.

Frequently Asked Questions

Is X2CrNiMo18-14-3 the same thing as 316L?

Both 1.4435 and 1.4404 fall within the UNS S31603 limits, so 1.4435 can be certified as 316L. They are not interchangeable in every case. 1.4435 is held at the upper end of Cr, Ni and Mo, which raises its PREN and lowers ferrite in welds. Where a specification calls out 1.4435, supplying 1.4404 is not acceptable.

What is 1.4435 BN2 and do I need it?

BN2 refers to Basler Norm BN 2, a works standard of the Basle chemical industry setting a restricted analysis aimed at keeping delta ferrite below 0.5 %. The standard was withdrawn without replacement in 2012, but the major mills kept 1.4435 BN2 in their programmes. Current industry guidance is that ferrite control at 0.5 % max in welds is generally not necessary for pharmaceutical plant. Orbital welds in 1.4435 BN2 average about 3 % delta ferrite, and a measurable drop in pitting resistance has only been shown from roughly 5 % upward. Solution annealed wrought 316L material typically shows 0 to 3 vol% ferrite in any case.

Can you supply dual certified 316 / 316L forgings?

Yes, where the heat analysis and the mechanical results satisfy both grades. State the governing standard, for example ASTM A182 F316/F316L or EN 10222-5 1.4435, at enquiry stage so the melt, the forging reduction and the testing plan are set up correctly from the start.

What tolerances and machining allowance do you work to?

Parts are forged to drawing in as-forged, rough machined or finish machined condition. Send the drawing or a sketch with the finished dimensions and we will propose the forging envelope, the machining allowance and the ultrasonic acceptance class suited to the section.

What should an enquiry contain?

Grade and standard, product form, finished dimensions or drawing, quantity, delivery condition, certificate level under EN 10204, any NDT or corrosion test requirement, and the destination port. With that we can normally return a quotation within one working day.

Request a Quotation for X2CrNiMo18-14-3 Forgings

Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel +86-189-2135-9659  |  E-mail sales@steelforgepieces.com

Send the drawing or the size of the part you need, whether rings, rolled rings, flanges, bars, discs, shafts, sleeves, tube sheets or forged pipes, and we will quote our best price with EN 10204 3.1 or 3.2 certification.

Email the Forging Team

Technical data compiled from EN 10088-3, EN 10222-5 and published mill data sheets for 1.4435. Values are given for guidance and are not a warranty of properties. The governing figures are those of the standard agreed in the order. Last reviewed .