X1CrNiMoCuN24-22-8 Forgings
EN 1.4652, UNS S32654, 654 SMO. Seamless rolled rings, forged rings, flanges, shafts, discs, tube sheets, sleeves and valve parts in super-austenitic 1.4652, melted and forged in one works by Jiangyin Jiangnan Metal Co., Ltd., Jiangyin, Jiangsu, China.
- Designation
- X1CrNiMoCuN24-22-8, also written X1CrNiMoCuN24.22.8
- Material number
- 1.4652
- Equivalent
- UNS S32654, trade name 654 SMO. ISO designation 4652-326-54-I
- Type
- Fully austenitic, super-austenitic. High molybdenum, high nitrogen
- Standards
- EN 10088-1, EN 10088-2, EN 10088-3, DIN EN 10088-3, ISO 15510
- Composition
- Cr 23.0–25.0, Ni 21.0–23.0, Mo 7.0–8.0, N 0.45–0.55, Mn 2.0–4.0, Cu 0.3–0.6, C max 0.020 per cent
- Density
- 8.0 g/cm³ (0.289 lb/in³)
- PREN
- About 57 by Cr + 3.3 Mo + 16 N. Some mills quote above 60 using a higher nitrogen factor
- Delivery condition
- Solution annealed and water quenched (+AT)
- Certification
- EN 10204 3.1, or 3.2 countersigned by a third party
- Supplied by
- Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. sales@steelforgepieces.com, +86 189 2135 9659
What the grade is
X1CrNiMoCuN24-22-8, material number 1.4652, is a fully austenitic stainless steel and one of the most highly alloyed grades listed in EN 10088. The designation carries the analysis: extra-low carbon, nominally 24 per cent chromium, 22 per cent nickel and 8 per cent molybdenum, with copper and nitrogen added deliberately. Manganese is held at 2 to 4 per cent so the steel can hold 0.45 to 0.55 per cent nitrogen in solution. That nitrogen keeps the structure austenitic at this alloy level and lifts the proof strength well above a standard 316L.
Enquiries for this grade usually arrive after 316L, 904L or 254 SMO have failed in service or been ruled marginal at the design stage. Outside Europe the same steel is bought as UNS S32654, normally under the trade name 654 SMO. For pitting, crevice corrosion and chloride stress corrosion cracking it sits at the top of the austenitic stainless steels, close to the nickel-base alloys.
Chemical composition
| Limit | C | Si | Mn | P | S | Cr | Ni | Cu | Mo | N |
|---|---|---|---|---|---|---|---|---|---|---|
| Min. | – | – | 2.00 | – | – | 23.0 | 21.0 | 0.30 | 7.0 | 0.45 |
| Max. | 0.020 | 0.50 | 4.00 | 0.030 | 0.005 | 25.0 | 23.0 | 0.60 | 8.0 | 0.55 |
Balance iron, roughly 38 to 46 per cent. Sulphur is capped at 0.005 per cent, low even for a stainless steel, to protect hot ductility during forging and to remove sulphide initiation sites in service.
Mechanical properties
| Condition | Rm MPa | Rp0.2 MPa | A long. % | Hardness HBW | KV2 long. J |
|---|---|---|---|---|---|
| Solution annealed, water quenched | 750–1000 | min. 430 | min. 40 | max. 310 | min. 100 |
Published typical values for solution annealed material sit above these minima, near 880 MPa tensile, 490 MPa proof, 45 per cent elongation and 90 J Charpy V-notch. Properties for heavier forged sections are agreed case by case. Test location, orientation and sampling frequency are fixed at order entry.
Typical physical properties at 20 C
| Property | Metric | Imperial |
|---|---|---|
| Density | 8.0 g/cm³ | 0.289 lb/in³ |
| Elastic modulus | 210 GPa | 30 x 10⁶ psi |
| Shear modulus | 81 GPa | 12 x 10⁶ psi |
| Poisson ratio | 0.28 | 0.28 |
| Thermal conductivity | 9.8 W/m.K | 5.7 BTU/h.ft.F |
| Specific heat | 460 J/kg.K | 0.11 BTU/lb.F |
| Thermal expansion | 15 µm/m.K | 8.3 µin/in.F |
| Melting range | 1410–1460 C | 2560–2650 F |
Thermal conductivity is low even against other austenitic stainless steels. It governs heat exchanger and tube sheet detailing, and it sets the heating rates used on heavy sections.
Equivalent grades
| System | Designation |
|---|---|
| EN / DIN name | X1CrNiMoCuN24-22-8 |
| EN / DIN number | 1.4652 |
| UNS, USA | S32654 |
| Trade name | 654 SMO |
| ISO 15510 | 4652-326-54-I |
| China | 015Cr24Ni22Mo8Mn3CuN. S32652 appears in some cross-reference tables |
| Product standards | ASTM A312, A213, A249 as S32654. EN 10216-5, EN 10217-7 as 1.4652 |
Cross-references are guidance. The very high alloy super-austenitics began as proprietary grades, so regional equivalents are not always chemically identical. State the governing standard and grade on the enquiry and we confirm what can be certified.
Corrosion resistance
Performance comes from 7 to 8 per cent molybdenum combined with about 0.5 per cent nitrogen and 24 per cent chromium. Using the pitting index PREN = Cr + 3.3 Mo + 16 N, the nominal analysis gives roughly 57. Suppliers applying a nitrogen coefficient of 30 publish figures above 60. On either calculation 1.4652 ranks ahead of 254 SMO and 904L for pitting and crevice attack in hot seawater and concentrated chloride brines. It is also specified for sulphuric acid, organic acids and mixed acids carrying chloride ions at higher pressure and temperature, and for media that are oxidising and chloride bearing at once, such as chlorine dioxide service.
Forging, heat treatment, fabrication
Hot working
Forged between 1095 and 1205 C. The steel is strong at temperature and less forgiving than a standard austenitic, so reheats, die temperature and reduction per pass are planned to hold the finishing temperature.
Solution annealing
From 1150 C minimum, water quenched, to restore the fully austenitic structure and return nitrogen and molybdenum to solution.
Sigma phase
Precipitation can occur roughly between 700 and 900 C. Time in that band during forging, straightening and welding is held to the minimum the process allows.
Welding
Nickel-base filler metals such as Alloy 625, so the weld metal is not less corrosion resistant than the parent material.
Melting route
EF and LF with vacuum oxygen decarburisation for nitrogen and carbon control. ESR remelted material where the specification or the end user calls for it.
Inspection
Ultrasonic examination to EN 10228-3, SEP 1921 or ASTM A388 as specified, with EN 10204 3.1 certification or third party 3.2.
Product forms and size envelope
| Product form | Typical use |
|---|---|
| Seamless rolled rings | Pressure vessel and heat exchanger shell courses, girth rings, retaining rings |
| Forged rings | Sections and alloys outside the ring-mill envelope, upset and punched |
| Flanges, blinds, hubs | Seawater, firewater and subsea pipework, risers and manifolds |
| Round bars, hollow bars | Machined valve stems, spindles, fasteners, pump shafts |
| Shafts and spindles | Pumps, agitators and compressors in chloride or acid duty |
| Discs, tube sheets, covers | Shell and tube heat exchangers, brine heaters, condensers, valve discs |
| Sleeves, bushings, bodies | Valve bodies and seat rings for ball, gate, globe, check and plug valves |
| Nozzles, manifolds, blocks | Pressure parts, subsea connector bodies, custom machined components |
| Dimension | Limit | Set by |
|---|---|---|
| Rolled ring OD | up to 6,000 mm | 6 m radial-axial ring mill |
| Machined disc diameter | up to 5,000 mm | 5,000 mm vertical turning lathe |
| Shaft turned length | up to 14,000 mm | C61160 horizontal lathe, 15 m well furnace for vertical quench |
| Bored cylinders | 1,600 mm dia x 10,000 mm | CNC deep-hole drilling machine |
| Single-piece weight | up to 30,000 kg | 60 t maximum heat, 6,300 t press |
| Minimum order | 10 kg, no minimum piece count | Works policy |
| Lead time | 20 to 60 days | Route and heat treatment cycle |
These are plant limits across all grades. For 1.4652 the practical ceiling is normally set by ingot availability rather than press capacity, so the achievable size is confirmed against the drawing at enquiry.
Applications
Seawater desalination
Brine heater internals, high pressure brine recirculation piping, high pressure RO components and seawater piping in MSF and MED plants.
Offshore oil and gas
Seawater, firewater and subsea pipework with the associated risers, manifolds, pressure vessels, valves and heat exchangers, and produced-water handling.
Chemical process plant
Equipment exposed to sulphuric acid, organic acids and mixed chloride bearing acids in the higher pressure and temperature ranges.
Chlor-alkali and ClO2
Process piping, heat exchanger parts and valve components where oxidising conditions and high chloride levels occur together.
Power and FGD
Flue gas desulphurisation systems and waste incineration plant handling acidic chloride condensates.
Pulp and paper
Black liquor evaporator components in kraft mills, where alkaline chloride conditions crack lower alloyed steels.
Quotation
Send the drawing or the finished dimensions, the quantity, the governing standard, the delivery condition and the NDT and certification level required. Forged weight, machining allowance, heat treatment and test scope are quoted together, so the figure covers a part that can be accepted rather than a billet price.
Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town
Jiangyin City, Jiangsu Province, China
Tel +86 189 2135 9659
Email sales@steelforgepieces.com
Questions
Is X1CrNiMoCuN24-22-8 the same as 1.4652 and 654 SMO?
Yes. X1CrNiMoCuN24-22-8 is the EN chemical designation and 1.4652 the EN material number for the same steel. UNS S32654, trade name 654 SMO, is the recognised equivalent. Some Chinese tables list S32652 and 015Cr24Ni22Mo8Mn3CuN next to this grade, so confirm the exact specification on the order.
Can 1.4652 rings and flanges be forged to our drawing?
Yes. Rings and flanges are produced as open-die forgings or as seamless rolled rings depending on size and quantity, then solution annealed, machined to the agreed allowance, ultrasonically examined and certified to EN 10204 3.1 or 3.2.
Which welding consumable should be used?
Nickel-base fillers such as Alloy 625, so the weld metal is not the weak point for corrosion. Control heat input and time in the 700 to 900 C range to limit sigma phase.
How does it compare with 254 SMO (1.4547 / A182 F44)?
1.4652 carries 7 to 8 per cent molybdenum and 0.45 to 0.55 per cent nitrogen against the lower molybdenum and nitrogen of 254 SMO, giving higher pitting resistance in hot high-chloride media and a higher proof strength. 254 SMO remains the more economical choice where the service is less severe. See the A182 F44 / 254 SMO forgings page.
What sizes and weights can be supplied?
Plant limits are 6,000 mm outside diameter on the ring mill, 5,000 mm machined diameter, 14,000 mm shaft turning length, 1,600 by 10,000 mm bored, and 30,000 kg single-piece weight. For 1.4652 the ceiling is usually ingot availability, so the size is confirmed against the drawing. Minimum order 10 kg with no minimum piece count, normal lead time 20 to 60 days.
Related grades and sources
Enquiries for this grade are commonly compared against A182 F44 (254 SMO / 1.4547), 904L, Sanicro 28, Alloy 24, A182 F53 (2507 duplex), A182 F55, Alloy 31, Incoloy 825 and Hastelloy C-276.
Composition and specified mechanical properties are taken from the EN 10088-3 grade tables, with EN 10088-1, EN 10088-2 and ISO 15510 for designation and listing. Typical physical and mechanical values, the PREN calculation and the hot working and solution annealing ranges follow published mill and materials datasheets for 1.4652 and UNS S32654. Figures are given for reference and do not replace the agreed order specification or the material test certificate issued with the goods. A Markdown version of this page is published at /Stainless-Steel/X1CrNiMoCuN24-22-8.md. Page reviewed 9 October 2026.