Heat-resisting austenitic stainless steel
UNS S35315 Forgings EN 1.4854 / 353 MA. Seamless rolled rings, flanges, shafts, discs, bars, sleeves and tube sheets, forged to drawing.
UNS S35315 is an austenitic heat-resisting stainless steel with nominally 25 % chromium and 35 % nickel, alloyed with nitrogen and rare earth metals. It carries the European number 1.4854 and is sold commercially as 353 MA, a trademark owned by Outokumpu OY.
The grade exists for one job: high temperature service. High silicon plus a cerium addition give very high oxidation resistance and good scale adhesion under thermal cycling, with a maximum service temperature in air of 1150 °C (2102 °F). Nickel content and a dense chromium oxide also give good resistance to carburisation and nitrogen pick-up.
Jiangyin Jiangnan Metal Co., Ltd. melts and forges this grade in one works at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Telephone +86 189 2135 9659, email sales@steelforgepieces.com.
Check the grade against the duty before you order. UNS S35315 contains no molybdenum, and its maximum temperature for aqueous corrosion service is around 450 °C. It is not a seawater or acid grade. For firewater, subsea pipework or sulphuric acid duty, use a super duplex or high-alloy austenitic instead: see A182 F55, A182 F53 or 904L. Tell us the service conditions on your enquiry and we will say so if the grade on the drawing is wrong for the job.
Designations and standards
| System | Designation |
|---|---|
| UNS | S35315 |
| EN number | 1.4854 |
| Trade name | 353 MA (trademark of Outokumpu OY) |
| Mill product standards | ASTM A240 plate and sheet, ASTM A312 pipe, EN 10297-2 |
Sources: Alleima 353 MA datasheet (UNS, EN number, product standards, trademark note).
No dedicated forging specification lists this grade, so forgings are supplied against the composition and property limits of the standard agreed at order entry. Name the governing standard on your enquiry and the certificate will be issued to it.
Chemical composition
| Element | Nominal |
|---|---|
| Carbon, C | 0.07 |
| Silicon, Si | 1.6 |
| Manganese, Mn | 1.5 |
| Phosphorus, P | ≤ 0.040 |
| Sulphur, S | ≤ 0.015 |
| Chromium, Cr | 25 |
| Nickel, Ni | 35 |
| Nitrogen, N | 0.16 |
| Cerium, Ce | 0.05 |
| Iron, Fe | Balance |
Nominal values: Alleima 353 MA datasheet. The ASTM A240 UNS S35315 data sheet published by Gravity Cast India lists cerium 0.030 to 0.100 %, balance iron.
Cerium enters the melt as misch metal containing roughly 50 % Ce, so the quantity of other rare earth metals is added to the cerium figure when checking a certificate.
A note on the cerium figure. A widely copied table lists cerium in this grade as 1.3 %, which duplicates the silicon value in the row above it. The real content is 0.030 to 0.100 %, roughly one fortieth of that. If a mill certificate shows 1.3 % Ce, query it before accepting the material.
Mechanical properties
Minimum values at room temperature
| Property | Metric | Imperial |
|---|---|---|
| Proof strength Rp0.2 | ≥ 300 MPa | ≥ 44 ksi |
| Proof strength Rp1.0 | ≥ 340 MPa | ≥ 49 ksi |
| Tensile strength Rm | ≥ 650 MPa | ≥ 94 ksi |
| Elongation A (5.65√S₀) | ≥ 40 % | ≥ 40 % |
| Elongation A2" | ≥ 35 % | ≥ 35 % |
| Hardness, Vickers | approx. 160 | approx. 160 |
Alleima 353 MA datasheet. The A240 sheet published by Gravity Cast India gives the same 650 MPa tensile and 40 % elongation minima.
Typical annealed values
Typical rather than guaranteed figures reported for the annealed grade are 720 to 740 MPa tensile strength (104,000 to 110,000 psi), 300 to 360 MPa yield strength (44,000 to 52,200 psi), 46 to 50 % elongation at break, and Brinell hardness around 190. Buy against the minima in the table above and treat these as indicative only.
AZoM grade 353MA datasheet (720 MPa, 360 MPa, 50 %); MakeItFrom UNS S35315 (740 MPa, 300 MPa, 46 %, 190 HB).
Short-term strength at temperature
| °C | Rp0.2, MPa | Rp1.0, MPa | Rm, MPa |
|---|---|---|---|
| 100 | 228 | 261 | 536 |
| 200 | 195 | 223 | 498 |
| 300 | 166 | 190 | 470 |
| 400 | 152 | 173 | 444 |
| 500 | 143 | 163 | 437 |
| 600 | 138 | 159 | 422 |
Creep data, average values
| °C | 1 %, 10,000 h | 1 %, 100,000 h | Rupture, 10,000 h | Rupture, 100,000 h |
|---|---|---|---|---|
| 550 | 149 | 86 | 206 | 129 |
| 600 | 88 | 52 | 127 | 80 |
| 650 | 54 | 33 | 82 | 52 |
| 700 | 35 | 21 | 56 | 36 |
| 750 | 22 | 14 | 39 | 25 |
| 800 | 15 | 9.7 | 28 | 18 |
| 850 | 10.5 | 6.9 | 20 | 14 |
| 900 | 8 | 5.1 | 15 | 10 |
| 950 | 6 | 3.9 | 11 | 6.7 |
| 1000 | 4.5 | 3.0 | 8 | 4.8 |
| 1050 | 3.5 | 2.3 | 6 | 3.5 |
| 1100 | 2.7 | 1.8 | 4.5 | 2.9 |
Elevated temperature and creep data: Alleima 353 MA datasheet. Average values, published for seamless tube. Use for comparison only; design values must come from the governing design code.
Physical properties
| °C | Thermal cond., W/m·°C | Specific heat, J/kg·°C | Modulus, GPa | Resistivity, µΩ·m |
|---|---|---|---|---|
| 20 | 11 | 480 | 190 | 1.00 |
| 200 | 15 | 530 | 180 | 1.07 |
| 400 | 18 | 575 | 165 | 1.14 |
| 600 | 22 | 610 | 155 | 1.20 |
| 800 | 25 | 640 | 140 | 1.25 |
| 1000 | 27 | 665 | 130 | 1.30 |
| 1100 | 29 | 680 | 125 | 1.32 |
Mean thermal expansion is 15.5 × 10⁻⁶ /°C over 20 to 100 °C, rising to 18 × 10⁻⁶ /°C over 20 to 1000 °C. Melting range is 1330 to 1370 °C.
Alleima 353 MA datasheet; melting range from MakeItFrom UNS S35315.
Behaviour at high temperature
Oxidation resistance comes from the high silicon content together with the rare earth metal addition. The rare earth addition also improves scale adhesion during temperature cycling, which in practice means less spalling in furnaces that are repeatedly heated and cooled.
Because the alloy forms a dense chromium oxide and carries 35 % nickel, it also resists carburisation and nitrogen pick-up. In cracked ammonia testing its nitrogen pick-up resistance was similar to Alloy 601. High nickel alloys are generally sensitive to sulphur attack at temperature, but under oxidising conditions the protective oxide forms and sulphur resistance improves.
Maximum service temperature in air is 1150 °C (2102 °F). One point matters when planning service: operation below 950 °C (1742 °F) may reduce room temperature impact toughness, so the grade is better suited to continuous high temperature duty than to long holds in the intermediate range.
Alleima 353 MA datasheet (oxidation, carburisation, nitriding, sulphur); AZoM grade 353MA (service temperature limits).
Heat treatment, welding and forming
Heat treatment
Solution annealing is carried out at 1100 to 1200 °C (2010 to 2190 °F) for 5 to 20 minutes, followed by rapid cooling in air or water. Where stress relief is required, 1000 to 1100 °C for 10 to 15 minutes with air cooling is recommended. Forgings leave this works solution annealed unless the order states otherwise.
Welding
Weldability is good. Manual metal arc and gas shielded arc welding both suit the grade, with TIG as first choice. Like all fully austenitic stainless steels it has low thermal conductivity and high thermal expansion, so the welding sequence should be planned in advance to limit distortion. Heat input below 1.0 kJ/mm and interpass temperature below 100 °C (210 °F) are recommended. Where residual stress is a concern, solution anneal after welding.
| Process | Consumable |
|---|---|
| TIG / GTAW, MIG / GMAW | ISO 18274 S Ni 6082 / AWS A5.14 ERNiCr-3 |
| MMA / SMAW | ISO 14172 E Ni 6182 / AWS A5.11 ENiCrFe-3 |
Cold forming
The grade is stronger than conventional stainless steels, so cold bending needs higher deformation forces. Annealing after cold bending is not normally necessary, but the degree of bending and the service conditions should decide that.
Heat treatment, welding parameters, filler metals and bending: Alleima 353 MA datasheet.
Where the grade is used
Documented application areas are high temperature petrochemical and furnace equipment:
- Ethylene furnace radiant cracking tubes
- EDC furnace tubes
- Waste heat recovery systems in the metallurgical industry, for example recuperators
- Heat treatment furnace internals: muffle tubes, radiant tubes, thermocouple protection tubes, burner components, furnace rollers
- Recuperator tubes in chemical waste and sewage sludge incineration
- Components requiring heat and creep resistance above 550 °C in the iron, steel and non-ferrous industries, the cement industry, engineering and energy conservation plant
Alleima 353 MA datasheet; AZoM grade 353MA.
What we forge against those duties
Seamless rolled rings and retaining rings for furnace rollers and burner assemblies. Flanges and tube sheets for recuperators and waste heat exchangers. Round bars, shafts and spindles for furnace roller and conveyor drives. Discs, blanks and sleeves for burner and muffle components. Bushings, nozzles and thermocouple protection hardware. Open-die forging and ring rolling cover most axisymmetric and blocky shapes, so send the drawing if the part you need is not on that list.
Forging, testing and certification
Steel for this grade is melted and refined on site through the electric arc furnace, ladle furnace and vacuum oxygen decarburisation route, with electroslag remelting available where the order calls for it. Because the works melts its own steel, the certificate traces a finished part back to its melt number rather than stopping at a purchased billet.
Forgings are ultrasonically examined to EN 10228-3, SEP 1921 or ASTM A388 at the acceptance class you nominate, and certified to EN 10204 3.1, or 3.2 with third party attendance. Mechanical testing, intergranular corrosion testing, PMI and dimensional reports are available on request. State the standard, acceptance class and any test temperature on the enquiry so the quotation covers the real scope of work.
| Item | Detail |
|---|---|
| Product forms | Seamless rolled rings, forged rings, flanges, shafts, discs, tube sheets, bars, blocks, sleeves, bushings, nozzles |
| Condition | Solution annealed, rough machined or proof machined as ordered |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days depending on size and test scope |
| NDT | EN 10228-3, SEP 1921, ASTM A388 |
| Certification | EN 10204 3.1 or 3.2 |
Questions we get asked
What is UNS S35315?
An austenitic heat-resisting stainless steel with nominally 25 % chromium and 35 % nickel, alloyed with nitrogen and rare earth metals. European number 1.4854. Sold commercially as 353 MA, a trademark owned by Outokumpu OY.
How much cerium does it contain?
0.030 to 0.100 %, with 0.05 % as the nominal figure. The cerium goes in as misch metal containing about 50 % Ce, so other rare earth metals count toward the total. Tables showing 1.3 % repeat a copying error.
What is the maximum service temperature?
1150 °C (2102 °F) in air. Service below 950 °C may reduce room temperature impact toughness.
Can it be used in seawater or sulphuric acid?
No. There is no molybdenum in the composition and the maximum temperature for aqueous corrosion service is around 450 °C. Use a super duplex grade such as A182 F53 or F55, or a high-alloy austenitic such as 904L, for those duties.
Which filler metal should be used?
ERNiCr-3 (ISO 18274 S Ni 6082) for TIG and MIG. ENiCrFe-3 (ISO 14172 E Ni 6182) for manual metal arc. Keep heat input under 1.0 kJ/mm and interpass temperature under 100 °C.
What do you need in order to quote?
A drawing or the finished dimensions with machining allowance, the governing standard, quantity, certification level, NDT standard and acceptance class, and any supplementary testing. Send it to sales@steelforgepieces.com and you will get price and lead time back.
Request a price for UNS S35315 forgings
Send a drawing or the finished dimensions. If the service conditions suggest a different grade would do the job better or cheaper, we will say so.
- Company
- Jiangyin Jiangnan Metal Co., Ltd.
Open-die forging works, established 1997 - Plant
- No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
- Telephone
- +86 189 2135 9659
Data sources
Figures on this page are drawn from the Alleima 353 MA material datasheet, the AZoM datasheet for stainless steel grade 353MA, the MakeItFrom entry for UNS S35315, and the ASTM A240 UNS S35315 data sheet published by Gravity Cast India. Where sources disagree, the mill datasheet minima are shown as governing and the rest are labelled typical. Data is given for comparison and does not replace the governing design code or a mill certificate.
353 MA is a trademark owned by Outokumpu OY. Alleima, Inconel, Incoloy, Hastelloy, Monel, Nimonic, Nitronic and other names used on this site belong to their respective owners. Jiangyin Jiangnan Metal Co., Ltd. is an independent forging manufacturer with no affiliation to these trademark holders. Grade names are used only to identify material specifications.