Titanium-stabilised austenitic stainless steel
UNS S31635 Forgings 316Ti and EN 1.4571. Rings, rolled rings, flanges, bars, shafts, discs, tube sheets and bored cylinders, forged from steel melted in our own furnaces.
UNS S31635 carries a nominal 16Cr-12Ni-2Mo-Ti composition. Titanium of at least five times the combined carbon and nitrogen content binds both elements as Ti(C,N), which keeps chromium in solution at the grain boundaries instead of letting it form chromium carbides. The practical result is that welds and parts held in the 450 to 850 C range keep their intergranular corrosion resistance without a post-weld anneal.
- UNS
- S31635
- EN number
- 1.4571
- EN name
- X6CrNiMoTi17-12-2
- AISI type
- 316Ti
- Structure
- Austenitic, non-magnetic as annealed
- Tensile min
- 515 MPa / 75 ksi
- Yield min
- 205 MPa / 30 ksi
- Elongation min
- 40 percent
- Hardness max
- 217 HB
- PREN
- 24 to 26
What you are buying
Jiangyin Jiangnan Metal Co., Ltd. is an integrated melting works and open-die forge at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, operating since 1997 with 460 staff. Most forging suppliers in China buy billet. This plant starts at the furnace: steel is melted and refined on site in a 25 t electric arc furnace with 25 t and 50 t ladle furnaces and 30 t and 60 t vacuum oxygen decarburisation units, with vacuum induction, vacuum arc and protective-atmosphere electroslag routes for the cleaner grades. Maximum heat size is 60 tonnes.
For S31635 that matters in two ways. The titanium window can be aimed at the forging the heat will become rather than accepted as delivered, and the certificate traces the part back to its melt number instead of stopping at a purchased billet. Forging runs on 6,300 t, 4,000 t and 2,000 t presses and three radial-axial ring mills, heat treatment on 14 furnaces, and machining on vertical lathes to 5,000 mm swing, all inside the same works. Heaviest single piece is 30 tonnes. The works holds CCS, BV, DNV, LR and NK approvals.
- Press
- 6,300 t
- Ring mill
- 6,000 mm OD
- Max single piece
- 30 t
- Max heat
- 60 t
- Minimum order
- 10 kg
- Lead time
- 20 to 60 days
Equivalent designations
The designations below describe the same titanium-stabilised 316 variant, but they are not numerically interchangeable. The EN grade runs a narrower molybdenum band and a tighter sulphur limit than the ASTM grade, so name the governing specification on the order rather than relying on the equivalence.
| System | Designation | Specification |
|---|---|---|
| UNS | S31635 | Unified Numbering System |
| ASTM | Type 316Ti | A240 / A240M, plate, sheet and strip |
| ASME | SA-240 Grade 316Ti | SA-240 / SA-240M |
| ASTM bar | 316Ti | A276, with A479 and SA-479 for vessel bar |
| EN number | 1.4571 | EN 10088-2 and 10088-3 delivery conditions |
| EN name | X6CrNiMoTi17-12-2 | EN 10028-7, pressure flat products |
| JIS | SUS 316Ti | JIS G4305 |
| AFNOR | Z6 CNDT 17-12 | NF EN 10088-3 |
| BS | 320S31 | BS 1501-3 |
| GB, China | 06Cr17Ni12Mo2Ti | National standard designation |
| GOST | 08Ch17N13M2T, 10Ch17N13M2T | Russian designation |
| PN | H17N13M2T | Polish designation |
| CSN and STN | 17 348 | Czech and Slovak designation |
Chemical composition
Titanium is the element that defines the grade. ASTM sets it as a minimum of five times the combined carbon and nitrogen content with a 0.70 percent ceiling, which is what guarantees the carbon is tied up rather than left free to form chromium carbides. Mills aiming for full stabilisation normally run a titanium to carbon ratio well above the minimum, and carbon is usually held under the 0.08 percent ceiling to limit excess titanium carbide.
| Element | ASTM A240 and ASME SA-240 Type 316Ti | EN 1.4571 |
|---|---|---|
| Carbon, C | 0.08 max | 0.08 max |
| Manganese, Mn | 2.0 max | 2.0 max |
| Silicon, Si | 0.75 max | 1.0 max |
| Phosphorus, P | 0.045 max | 0.045 max |
| Sulphur, S | 0.030 max | 0.015 max |
| Chromium, Cr | 16.0 to 18.0 | 16.5 to 18.5 |
| Nickel, Ni | 10.0 to 14.0 | 10.5 to 13.5 |
| Molybdenum, Mo | 2.0 to 3.0 | 2.0 to 2.5 |
| Nitrogen, N | 0.10 max | not specified |
| Titanium, Ti | 5 x (C+N) min, 0.70 max | 0.70 max |
| Iron, Fe | Balance | Balance |
The composition table on the previous version of this page carried a column headed N with a value of 0.50 max and a stray Ti entry. Those figures were wrong and have been replaced with the specification limits above. Every order ships with the actual heat analysis on the certificate.
Mechanical and physical data
Room-temperature minima apply in the solution-annealed condition. Titanium stabilisation keeps the properties in place after high-temperature exposure, which is the reason the grade is specified for thermally cycled parts rather than for a strength advantage over plain 316.
| Property | At 20 C | At 600 C |
|---|---|---|
| Tensile strength | 515 MPa / 75 ksi min | 380 MPa / 55 ksi min |
| Yield strength, 0.2 percent proof | 205 MPa / 30 ksi min | 160 MPa / 23 ksi min |
| Elongation | 40 percent min | 35 percent min |
| Reduction of area | 50 percent min | not specified |
| Hardness | 217 HB max | not specified |
| Modulus of elasticity | 193 GPa | 165 GPa |
| Thermal conductivity | 14.6 W/m.K | not specified |
| Coefficient of thermal expansion | 16.5 x 10-6 per C | not specified |
Allowable stress
| Temperature | 100 C | 300 C | 500 C | 600 C | 700 C |
|---|---|---|---|---|---|
| Allowable stress, MPa | 138 | 115 | 96 | 85 | 65 |
| Allowable stress, ksi | 20.0 | 16.7 | 13.9 | 12.3 | 9.4 |
Use the allowable stress from the applicable edition of the code for design. The figures above are for comparison between grades, not a substitute for the code table that governs your vessel.
Corrosion behaviour
The 2 to 3 percent molybdenum gives the same pitting and crevice resistance as 316 and 316L, with a PREN of 24 to 26 and a critical pitting temperature around 30 C by ASTM G48. Published service data puts the practical limit at roughly 2,000 ppm chloride. Titanium adds what the plain grades lack: the weld zone and the heat-affected zone stay resistant to intergranular attack, and material will pass ASTM A262 Practice E even after an hour at 700 C.
The grade was developed in the 1960s to deal with polythionic acid stress corrosion cracking in refineries and with sensitisation in welded 316, and that is still where it earns its place. It resists atmospheric and mild corrosion better than the 18Cr-8Ni grades and is more resistant than other chromium-nickel types to sulphuric acid solutions.
Two limits are worth stating plainly. Titanium stabilisation does not make the steel immune to chloride stress corrosion cracking, so hot chloride service still needs assessment, and a duplex or super-austenitic grade may be the better answer. For a chloride pitting upgrade, look at 904L or a duplex grade such as UNS S32900. For severe acid duty, the alloys in our nickel alloy range are the usual route.
Heat treatment, welding and machining
- Annealing. Heat from 1010 to 1120 C and cool rapidly in air or water. Best corrosion resistance is obtained when the final annealing temperature is above 1070 C.
- Stress relieving. Heat from 200 to 400 C and air cool.
- Hardening. Not possible by heat treatment. Strength is raised only by cold work.
- Sensitisation range. 450 to 850 C. This is the band the titanium addition is there to protect against, and the reason the grade suits intermittent heat and thermal cycling.
- Welding. ER316Ti or ER316L filler by GTAW or SMAW. Low heat input, around 1.0 to 1.5 kJ/mm, limits titanium loss. No preheat and no post-weld anneal are needed for most joints, and the weld keeps base-metal corrosion resistance.
- Machining. Not a free-machining grade, and not recommended for aggressive high-speed machining. Use rigid setups, sharp tooling and generous coolant. Titanium carbides and a work-hardening austenitic matrix are what make it demanding.
- Magnetic response. Non-magnetic as annealed. Cold work induces under about 10 percent martensite and a slight magnetic response, which full annealing removes. Worth telling your inspector before the part arrives.
- Upper temperature. ASME Section VIII Division 1 allows SA-240 316Ti to a maximum design temperature of 815 C. Oxidation data for the grade gives continuous service to about 870 C and intermittent service to about 925 C. Design pressure parts to the code value.
Forged shapes and size envelope
Every item is forged from a single piece of steel melted on site. No welding, no casting, no purchased billet of unknown origin. Size limits are set by the equipment listed against them.
| Product | Size limit | Set by |
|---|---|---|
| Seamless rolled rings | up to 6,000 mm outside diameter | 6 m radial-axial ring mill |
| Small and mid-range rings | from 50 mm outside diameter | Upset and punch route, 1 m and 3 m mills |
| Flanges | to ASME B16.5, B16.47 and API 6A | Press and ring mills |
| Shafts and spindles | up to 14,000 mm turned length | C61160 lathe, 15 m well furnace for vertical quench |
| Discs, tube sheets, blocks | up to 5,000 mm machined diameter | 5,000 mm vertical turning lathe |
| Bored cylinders, sleeves, bushings | up to 1,600 mm dia by 10,000 mm | CNC deep-hole drilling machine |
| Bars, flats and blocks | press capacity | 6,300 t, 4,000 t and 2,000 t presses |
| Single-piece weight | up to 30,000 kg | 60 t heat size and 6,300 t press |
Valve and wellhead parts are a regular order in this grade: bodies, bonnets, blocks, stems, seat rings, spools, nozzles and manifolds, including work to API 6A and NACE MR0175 or ISO 15156 where the specification calls for it.
Where it is used
S31635 is specified where 316-level corrosion resistance has to survive welding and heat without a post-weld anneal. Typical duties:
- Petrochemical and refining. Heat exchangers, catalytic recovery systems and recuperators, where resistance to polythionic acid cracking is the reason for the grade.
- Power generation. Boiler and superheater components held at temperature for long periods.
- Chemical process plant. Acid reactors, chemical transport containers and process vessels seeing chloride and heat together.
- Pulp and paper. Digesters, liquor tanks and paper machine components.
- Exhaust and thermal plant. Manifolds, ducting and thermal oxidisers under thermal cycling.
- Desalination. Evaporator components in seawater at temperature.
- Food, beverage and pharmaceutical. Process equipment in acidic environments, and laboratory and medical equipment.
- Oil and gas. Subsea and deepwater production parts, air compressors, power and nitrogen generators.
316Ti against 316L, 316 and 321
All four are cross-shopped. The choice turns on how carbon is controlled and whether molybdenum is present.
| Property | 316Ti, S31635 | 316L, S31603 | 316, S31600 | 321, S32100 |
|---|---|---|---|---|
| Type | Austenitic, Mo, Ti-stabilised | Austenitic, Mo, low carbon | Austenitic, Mo | Austenitic, Ti-stabilised |
| Carbon max | 0.08 | 0.03 | 0.08 | 0.08 |
| Chromium | 16.0 to 18.0 | 16.0 to 18.0 | 16.0 to 18.0 | 17.0 to 19.0 |
| Nickel | 10.0 to 14.0 | 10.0 to 14.0 | 10.0 to 14.0 | 9.0 to 12.0 |
| Molybdenum | 2.0 to 3.0 | 2.0 to 3.0 | 2.0 to 3.0 | none |
| Stabiliser | Ti, 5 x (C+N) min | none | none | Ti, 5 x C min |
| PREN | 24 to 26 | 24 to 26 | 24 to 26 | 18 to 20 |
| Yield min, MPa | 205 | 170 | 205 | 205 |
- 316Ti against 316L. 316Ti holds up under thermal cycling because the titanium carbides stay stable, and it carries a higher minimum yield, 205 against 170 MPa. 316L relies on low carbon and is the usual pick for ambient welded work and polished surfaces.
- 316Ti against 316. Similar strength. 316Ti is weld-stable without an anneal, which matters on thick sections.
- 316Ti against 321. Both are titanium-stabilised, but 321 has no molybdenum and a PREN of 18 to 20. Choose 316Ti for wet corrosion combined with heat, 321 for dry high-temperature oxidation.
Testing and certification
- Ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388, to the acceptance class you nominate, on PXUT-3300, USM35XS and CTS-22 flaw detectors.
- Chemical analysis by optical emission spectrometry to ASTM E415, with infrared carbon and sulphur analysis to ASTM E1019 and handheld positive material identification.
- Mechanical testing on 600 kN and 300 kN universal machines to ASTM A370 and ISO 6892. Charpy V-notch impact testing to minus 60 C in-house, lower temperatures through an accredited laboratory.
- Intergranular corrosion testing to ASTM A262 or ASTM G28 and pitting resistance to ASTM G48, placed with an accredited third-party laboratory and reported alongside the mill certificate.
- Magnetic particle inspection to ASTM E709 and metallographic grain size to ASTM E112 on site.
- Certification to EN 10204 3.1, or EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector. Works approvals: CCS, BV, DNV, LR and NK.
- Traceability from the melt number through forging, heat treatment and machining, because all of those steps happen inside one works.
Questions we get asked
What is UNS S31635?
A titanium-stabilised, molybdenum-bearing austenitic stainless steel of nominal 16Cr-12Ni-2Mo-Ti composition, designated 316Ti in the AISI system and 1.4571 or X6CrNiMoTi17-12-2 in EN. Titanium at a minimum of five times the combined carbon and nitrogen content binds both as Ti(C,N) and stops chromium carbide precipitation at grain boundaries during welding or exposure in the 450 to 850 C range.
Is UNS S31635 the same as 316Ti and 1.4571?
Same material, different limits. ASTM A240 Type 316Ti allows Cr 16.0 to 18.0, Ni 10.0 to 14.0, Mo 2.0 to 3.0 and S 0.030 max. EN 1.4571 specifies Cr 16.5 to 18.5, Ni 10.5 to 13.5, Mo 2.0 to 2.5 and S 0.015 max. Name the governing specification on the order.
What is the chemical composition?
To ASTM A240 and ASME SA-240: C 0.08 max, Mn 2.0 max, Si 0.75 max, P 0.045 max, S 0.030 max, Cr 16.0 to 18.0, Ni 10.0 to 14.0, Mo 2.0 to 3.0, N 0.10 max, Ti 5 x (C+N) min to 0.70 max, balance iron.
What are the mechanical properties?
Solution annealed at room temperature: tensile 515 MPa or 75 ksi minimum, 0.2 percent proof stress 205 MPa or 30 ksi minimum, elongation 40 percent minimum, reduction of area 50 percent minimum, hardness 217 HB maximum, modulus 193 GPa. At 600 C: 380 MPa tensile, 160 MPa yield, 35 percent elongation.
How is it heat treated after forging?
Anneal from 1010 to 1120 C with a rapid cool in air or water, taking the final annealing temperature above 1070 C for best corrosion resistance. Stress relieve from 200 to 400 C and air cool. The grade cannot be hardened by heat treatment.
Does it need post-weld heat treatment?
No. The titanium holds carbon and nitrogen as Ti(C,N), so the weld zone keeps its intergranular corrosion resistance without an anneal. Use ER316Ti or ER316L filler by GTAW or SMAW at low heat input, around 1.0 to 1.5 kJ/mm, to limit titanium loss. No preheat for most joints.
316Ti or 316L?
316L holds carbon to 0.03 percent maximum. 316Ti stabilises a 0.08 percent maximum with titanium. Pick 316Ti where the part is thermally cycled or held between 450 and 850 C, and note the higher minimum yield, 205 against 170 MPa. Pick 316L for ambient welded work and for polished or fine-surface components.
What is the maximum service temperature?
Two different numbers, for two different purposes. ASME Section VIII Division 1 allows SA-240 316Ti to a maximum design temperature of 815 C or 1500 F, and that is the figure to design pressure parts to. Oxidation data for the grade gives continuous service to about 870 C and intermittent service to about 925 C.
Is it magnetic?
Non-magnetic as annealed, since the structure is fully austenitic. Cold work induces under about 10 percent martensite and a slight magnetic response. Full annealing restores the non-magnetic condition.
Is it suitable for seawater?
The 2 to 3 percent molybdenum gives a PREN of 24 to 26 and a critical pitting temperature around 30 C, and the titanium keeps weld zones resistant, which is why the grade is used in desalination evaporators and offshore heat exchangers. It is not immune to chloride stress corrosion cracking, so hot chloride duty needs assessment against a duplex or super-austenitic alternative.
What is the minimum order and lead time?
Minimum order is 10 kg with no minimum piece count, so one-off prototypes and production batches are both accepted. Lead time runs 20 to 60 days depending on size, heat treatment and test scope.
Request a quotation
Send the drawing or the dimensions, the quantity, the governing specification and the test and certification scope you need. Price and lead time come back from the works, not from a trading desk. If the grade is not settled yet, send the service conditions instead and we will tell you what we would forge it in.
Business hours are Monday to Saturday, 08:00 to 17:30 China Standard Time, UTC+8. Customer audits, pre-shipment inspections and third-party witness testing are welcome. Arrange visits by email in advance so an English-speaking engineer is available.
- CompanyJiangyin Jiangnan Metal Co., Ltd.
- WorksNo.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
- Telephone+86 189 2135 9659
- Emailsales@steelforgepieces.com
- Websitewww.steelforgepieces.com
- Since1997, 460 staff, CCS BV DNV LR NK