UNS S31000 / Type 310 / ASTM A182 F310 / W.Nr. 1.4845 Melted and forged at one works, Jiangyin, China · +86 189 2135 9659 · sales@steelforgepieces.com
Jiangnan Metal Melting works · Open-die forge · Ring mill Get a price

Heat-resistant austenitic stainless steel

UNS S31000 forgings Type 310 rings, flanges, bars, discs and shafts, melted and forged at one works

UNS S31000 is Type 310 heat-resistant austenitic stainless steel, nominally 25 per cent chromium and 20 per cent nickel, with carbon up to 0.25 per cent. Ordered as forgings it is normally specified as ASTM A182 grade F310. The chromium and silicon give oxidation resistance to 1050 C in continuous service, resistance to sulphidation and usable life in moderately carburising atmospheres, while the fully austenitic structure stays tough down to -268 C with low magnetic permeability.

Jiangyin Jiangnan Metal Co., Ltd. melts this grade in its own electric arc furnace and VOD plant at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, then forges, ring-rolls, heat-treats, machines and tests it on the same site. Rings roll to 6000 mm outside diameter, single pieces reach 30 tonnes, and the minimum order is 10 kg.

Grade summaryS31000
UNS
S31000
Type
310 · A182 F310 · 1.4845
Chromium
24.0 to 26.0 per cent
Nickel
19.0 to 22.0 per cent
Carbon
0.25 per cent max
Hot range
1050 C continuous, 1100 C peak
Cold range
Tough to -268 C
Density
7.89 g/cm3
Certificate
EN 10204 3.1 or 3.2
01

310, 310S and 310H are three different UNS numbers

All three share the same 25Cr 20Ni base and differ in carbon. They are not interchangeable on a certificate, and writing S31000 and 310H on the same line of an enquiry is the most common ordering error on this grade. Carbon raises creep strength and lowers corrosion resistance after welding, so the choice has consequences in service.

Carbon and silicon limits, weight per cent, maximum unless a range is given
GradeUNSCarbonSiliconWhy it is chosen
310S310000.251.50General heat-resisting workhorse
310SS310080.081.50Low carbon, easier fabrication and welding
310HS310090.04 to 0.100.75Carbon held high and narrow for creep resistance
Ordering note

If your drawing says 310H we will melt to S31009 limits, not S31000, and the grain size requirement changes with it. Confirm the UNS number at enquiry stage. Changing it after the heat is cast means a new heat.

02

Chemical composition

For forged pressure parts the governing chemistry is ASTM A182 grade F310, listed in that specification as the 25 chromium 20 nickel alloy. Note the silicon column. A182 forgings are held to 1.00 per cent maximum, while Type 310 plate to ASTM A240 is allowed 1.50 per cent. Quoting the plate limit on a forging certificate is a routine cause of rejection at goods inwards. Typical silicon in the alloy sits near 0.6 per cent.

UNS S31000 to ASTM A182 grade F310, weight per cent
LimitCMnSiPSCrNiMoFe
Minimum–––––24.0019.00–Balance
Maximum0.252.001.000.0450.03026.0022.00Not specified

There is no deliberate molybdenum addition. That single fact decides most of the applications this grade should and should not be used for, and it is covered in section 06.

03

Mechanical properties

Two sets of figures get confused on supplier websites. The first is the acceptance minimum a forging has to meet under ASTM A182 F310. The second is what solution annealed material typically does at room temperature, which sits well above the minimum. Design to the minimum, expect the typical.

Room temperature properties: A182 F310 minima against typical annealed values
PropertyASTM A182 F310 minimumTypical, solution annealed
Tensile strength515 MPa (75 ksi)550 MPa (80 ksi)
Yield strength, 0.2 per cent offset205 MPa (30 ksi)245 MPa (35 ksi)
Elongation in 2 in. or 4D30 per cent45 per cent
Reduction of area50 per centNot quoted
HardnessNot mandated for austenitic grades in A182217 HB maximum

Creep

Most S31000 forgings work hot, so creep rather than room temperature tensile strength usually sets the section. Typical values follow.

Typical creep strain and creep rupture strength, MPa
TemperatureCreep strainCreep rupture
1 000 h10 000 h100 000 h1 000 h10 000 h100 000 h
600 C1201004020014080
700 C503520804520
800 C2010835208
900 C106315105
1000 C531.5942

Physical properties

Physical properties of alloy 310
PropertyMetricImperial
Density7.89 g/cm30.285 lb/in3
Modulus of elasticity196 GPa28.5 x 106 psi
Melting range1354 to 1402 C2470 to 2555 F
Specific heat, 0 to 100 C502 J/kg·K0.12 BTU/lb·F
Thermal conductivity10.8 W/m·K8.0 BTU/hr/ft2/ft/F
Electrical resistivity at 20 C78.0 microhm·cm30.7 microhm·in
04

Service temperature by atmosphere

The oxidation limit for this grade is not one number. It moves with the sulphur load and the oxygen potential of the gas, and quoting 1100 C for a furnace running dirty fuel will shorten the life of the part. Use the line that matches the real atmosphere.

Maximum service temperature of alloy 310
AtmosphereLimit
Oxidising, sulphur up to 2 g/m31050 C continuous service, 1100 C peak
Oxidising, sulphur above 2 g/m3950 C maximum
Low oxygen, sulphur up to 2 g/m31000 C maximum
Nitriding or carburising850 to 950 C maximum
CryogenicTough to -268 C, low magnetic permeability

In reducing, nitriding and carburising gas the alloy does not match Alloy 600 or Alloy 800, but it outperforms most heat-resisting stainless steels in those conditions.

05

Where UNS S31000 is used

Every item below is forged from one piece of steel melted on this site. No welding, no casting, no purchased billet of unknown origin.

Thermal processing

Annealing covers and boxes, muffles and retorts, burner grids, doors, fans, walking beams and recuperators. Forged rings, sleeves and bars.

Furnace parts

Burners, doors, fans, piping and recuperators, plus heat-treatment baskets and jigs where the frame has to survive repeated cycling.

Fluidised bed furnaces

Coal combustor internals, grids, piping and wind boxes. Forged discs and bars proof-machined for volumetric inspection.

Petroleum refining

Catalytic recovery system parts, flares, recuperators and tube hangers. Forged flanges and tube sheets for hot oxidising and sulphidising gas.

Power generation

Coal gasifier internals, pulverised coal burners and tube hangers. Forged discs, sleeves and shafts.

Sintering and cement

Burners and burner shields, feeding and discharging system parts, wind boxes.

Ore processing and steel plant

Smelter and steel melting equipment, continuous casting equipment. Rolls, crane wheels and heavy rings.

Cryogenic components

Forged rings and bodies where toughness to -268 C and low magnetic permeability are required.

Food processing

Equipment and storage components exposed to high temperature cleaning cycles.

Product forms

Forged and ring-rolled forms available in UNS S31000
FamilyItemsEnvelope
RingsSeamless rolled rings, forged rings, retaining rings, valve seat rings, gear ring blanksOD 50 to 6000 mm
Flanges and flat workWeld neck, blind, slip-on, socket weld and orifice flanges, tube sheets, covers, blocksTo 5000 mm machined diameter
Shafts and barsRound, flat and square bars, stepped shafts, eccentric shafts, spindles, gear shaftsTo 14 000 mm turned length
Hollow sectionsCylinders, sleeves, bushings, couplings, heavy-wall pipe bored from solidTo 1600 mm dia x 10 000 mm bored
Discs and wheelsForged discs, blanks, hubs, wheels, rollsTo 30 t single piece
Valve and vessel partsBodies, bonnets, stems, seat rings, nozzles, manifoldsForged from one piece, no welds
06

Where this grade is the wrong choice

Specifying 310 correctly means knowing what it cannot do. Most failures on this alloy trace back to one of the five points below rather than to anything that happened in the forge.

  • Wet or chloride corrosion. Alloy 310 is not designed for service in wet corrosive environments. The high carbon that gives creep strength is detrimental to aqueous corrosion resistance, and the alloy is prone to intergranular corrosion after long exposure at temperature. With no molybdenum, chloride pitting and crevice resistance is weak. For seawater, desalination, subsea or sour duty, specify A182 F44, duplex F51, F53 or F55, 904L or Incoloy 825.
  • Sigma phase. Between 650 and 950 C the alloy precipitates sigma phase and loses toughness. A solution anneal at 1100 to 1150 C restores a degree of it.
  • Severe carburising. The harsher carburising atmospheres in thermal process plant normally need a nickel alloy. Alloy 330, Inconel 600 or Incoloy 800H are the usual answers.
  • Cold forming before hot service. The alloy is ductile and cold forms much like 316, but cold forming parts destined for long term high temperature exposure is not recommended because of carbide and sigma phase precipitation.
  • Creep-critical duty. If the design is governed by creep, 310H (S31009) with its controlled carbon is the grade to specify, not S31000.
07

How we make it

Melting

Stainless grades run through the 25 t electric arc furnace, are refined in a 25 t or 50 t ladle furnace, and are decarburised under vacuum in the 30 t or 60 t VOD units where carbon and nitrogen have to be held tight. Protective-atmosphere electroslag remelting at 3 t or 6 t is available where cleanliness or segregation governs. Maximum heat size is 60 tonnes. Because the melt is on site, chemistry is aimed at the forging the steel will become rather than accepted as delivered, and traceability starts at the melt number instead of a purchased billet certificate.

Forging and heat treatment

Hot working is done between 950 and 1200 C after uniform through-heating, on 6300 t, 4000 t and 2000 t hydraulic presses, with radial-axial ring mills at 6 m, 3 m and 1 m. After hot forming, parts take a final anneal at 1000 to 1150 C followed by rapid quenching. Where sigma phase exposure has to be reversed, the anneal is run at 1100 to 1150 C. Fourteen heat-treatment furnaces are on site, including two 15 m deep well-type furnaces that let long shafts be quenched vertically rather than laid down.

Testing and paperwork

Inspection scope for UNS S31000 forgings
ItemMethod or standard
Chemical analysisOptical emission spectrometry to ASTM E415, infrared carbon and sulphur to ASTM E1019, handheld PMI on the finished part
Tensile and elongationASTM A370 or ISO 6892 on 600 kN and 300 kN machines, acceptance to A182 F310
Ultrasonic testingASTM A388 or SEP 1921. In European practice the part covering austenitic forgings is EN 10228-4, not EN 10228-3
SurfaceLiquid penetrant examination. Magnetic particle does not apply to this austenitic grade
Grain sizeASTM E112 metallography on site
Intergranular corrosionASTM A262 or ASTM G28, placed with an accredited third-party laboratory and reported alongside the mill certificate
CertificationEN 10204 3.1 as standard. EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector on request
Class approvalsCCS, BV, DNV, LR, NK

Supporting records supplied with the parts include heat-treatment charts, NDT reports, dimensional reports and PMI records.

08

Designations and standards

Cross-reference for UNS S31000. Confirm against the governing specification before ordering
SystemDesignation
UNSS31000
AISI type310
Werkstoff1.4845
ForgingsASTM A182 grade F310
Plate and flat productASTM A240, ASME SA240, AMS 5521
Related gradesS31008 (310S), S31009 (310H)
09

Questions we get asked

Is UNS S31000 the same as 310H?

No. UNS S31000 is Type 310, carbon 0.25 per cent maximum. 310H is UNS S31009, carbon held between 0.04 and 0.10 per cent for enhanced creep resistance. 310S is the low carbon version, UNS S31008, at 0.08 per cent maximum. Silicon differs too: 1.50 per cent for 310 and 310S against 0.75 per cent for 310H.

Jiangyin Jiangnan Metal forges all three. The UNS number has to be on the enquiry because the chemistry is fixed before the ingot is cast.

What is the chemical composition of UNS S31000 forgings?

To ASTM A182 F310: carbon 0.25 max, manganese 2.00 max, silicon 1.00 max, phosphorus 0.045 max, sulphur 0.030 max, chromium 24.00 to 26.00, nickel 19.00 to 22.00, balance iron, all weight per cent. Silicon is the trap. Forgings are held to 1.00 per cent while Type 310 plate to ASTM A240 is allowed 1.50 per cent.

What is the maximum service temperature?

In oxidising conditions with sulphur up to 2 g/m3, 1050 C continuous with a 1100 C peak. Above 2 g/m3 sulphur, 950 C. In a low oxygen atmosphere, 1000 C. In nitriding or carburising gas, 850 to 950 C. At the cold end the alloy stays tough to -268 C.

Can it be used in seawater or wet chloride service?

No. The alloy is not designed for wet corrosive environments, the high carbon works against aqueous corrosion resistance, and there is no molybdenum for chloride pitting resistance. It is also prone to intergranular corrosion after long high temperature exposure. Use A182 F44, duplex F51, F53 or F55, 904L or Incoloy 825 for those duties.

Which ultrasonic standard applies?

Type 310 is fully austenitic, so in European practice the applicable part is EN 10228-4, covering austenitic and austenitic-ferritic stainless steel forgings. EN 10228-3 is written for ferritic and martensitic forgings. ASTM A388 or SEP 1921 can be used where the order specifies them.

What sizes and weights can you forge?

Seamless rings to 6000 mm outside diameter on the 6 m radial-axial mill, with 3 m and 1 m mills below that and an upset-and-punch route for rings from 50 mm. Heaviest single forging 30 tonnes. Shafts turn to 14 m between centres and bores run to 1600 mm diameter by 10 000 mm deep. Minimum order 10 kg with no minimum piece count.

Do you melt the steel or buy billet?

We melt it. Electric arc furnace, ladle furnace and vacuum oxygen decarburisation for stainless grades, with electroslag remelting where cleanliness governs, up to 60 t heats. The certificate traces the part back to its melt number rather than to a billet bought in.

Is it weldable?

Yes, by TIG, plasma, MIG, SMAW, SAW and FCAW. Where corrosion resistance after welding matters, 310S is the better pick because it limits carbide precipitation in the heat affected zone.

What is the lead time?

20 to 60 days from order confirmation. Standard stainless grades melted through the arc furnace sit at the lower end. Anything needing a remelting step, third-party witnessed inspection or outside laboratory corrosion testing sits at the upper end. Flag witnessed inspection at enquiry stage so it is built into the quoted date.

10

Request a price

Quotations are prepared from a drawing or a written specification. Sending the six items below in the first email removes a round trip and usually gets a price back within two working days.

What to include in the enquiry
#ItemExample
1Grade or specificationUNS S31000 / ASTM A182 F310
2Dimensions, or a drawing in PDF, DWG, DXF or STEPOD 1400 x ID 1100 x H 240 mm
3Quantity and expected repeat volume8 pcs, about three times a year
4Delivery conditionAs-forged, proof-machined or finish-machined
5Heat treatment and testingSolution annealed, UT to ASTM A388, ASTM A262 Practice E
6Certification and destination portEN 10204 3.2 witnessed by DNV, Rotterdam

Telephone, WhatsApp and WeChat all reach the same number. Business hours are Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8). Minimum order 10 kg, no minimum piece count.

11

Related grades

Grades engineers commonly compare against S31000 when the service temperature, the atmosphere or the corrosion duty shifts.