GRADE UNS S13800 / PH13-8Mo / XM-13 / 1.4534 FORGINGS TO ASTM A705 · AMS 5629 Plain-text version

Precipitation hardening stainless steel

UNS S13800 Forgings Rings, seamless rolled rings, flanges, shafts, discs and bars in PH13-8Mo, forged to drawing

UNS S13800 is a martensitic precipitation hardening stainless steel containing 12.25 to 13.25 percent chromium, 7.50 to 8.50 percent nickel, 2.00 to 2.50 percent molybdenum and 0.90 to 1.35 percent aluminium. It carries high strength and hardness together with high toughness, good resistance to stress-corrosion cracking and little difference between longitudinal and transverse properties, which is why it is specified for heavy forged sections that cannot be tested in one direction only.

We melt this grade on site and forge it in the same works, so the certificate traces a finished part back to its melt number.

Grade dataS13800
Grade
UNS S13800
Also called
PH 13-8 Mo, 13-8 PH, alloy 13-8, XM-13, 1.4534, X3CrNiMoAl13-8-2
Forgings
ASTM A705 / ASME SA705
Bar, shapes
ASTM A564 / ASME SA564 Grade XM13
Aerospace
AMS 5629
Conditions
A, H950, H1000, H1025, H1050, H1100, H1150, H1150M, RH950
Melt route
VIM + VAR, ESR, or EAF + LF + VOD
Max piece
30,000 kg
Min order
10 kg, no minimum piece count
Lead time
20 to 60 days
01

What we forge in UNS S13800

Everything is forged from a single piece of steel. No welding, no casting, no billet of unknown origin.

Regular items in this grade are forged rings and seamless rolled rings, forged flanges, forged round bars and billets, forged shafts, spindles and eccentric shafts, forged discs, tube sheets and covers, forged sleeves, bushings and bored cylinders, and valve parts including bodies, bonnets, stems, seat rings and blocks. Rings come off the radial-axial mills up to 6,000 mm outside diameter, and below the ring-mill range we upset and punch instead, which takes ring sizes down to 50 mm outside diameter.

This is a premium grade, so we rarely hold it as stock sizes. Send the drawing or the finished dimensions with the required condition and we quote the forging weight, the machining allowance, the heat treatment and the testing as one price. Rough-machined and finish-machined parts both leave the same works, on vertical lathes up to 5,000 mm swing and horizontal lathes up to 14,000 mm between centres.

02

Designations and specifications

UNS S13800 cross-reference
System or product formDesignation
UNSS13800
ASTM and ASME gradeXM-13
EN material number1.4534
EN steel nameX3CrNiMoAl13-8-2
Shop namesPH 13-8 Mo, PH13-8Mo, 13-8 PH, alloy 13-8, 13-8 Mo
ForgingsASTM A705 / ASME SA705
Bar, wire, shapesASTM A564 / ASME SA564 Grade XM13
Bar, wire, forgings, rings, extrusionsAMS 5629, Type 1
Sheet, strip, plateASTM A693 / ASME SA693, AMS 5864

ASTM B564 is sometimes written on enquiries for this grade. B564 covers nickel-alloy forgings and does not list UNS S13800. For a stainless precipitation hardening forging the right reference is ASTM A705 Grade XM-13, or AMS 5629 where the part is aerospace work.

03

Chemical composition

Composition limits in weight percent, UNS S13800 type analysis
LimitCSiMnPSCrMoNiAlNFe
Min—————12.252.007.500.90—Bal.
Max0.050.100.100.0100.00813.252.508.501.350.010—

What separates this grade from the older precipitation hardening stainless steels is not the chromium and nickel but the restrictions on everything else. Silicon and manganese are held to 0.10 percent, phosphorus to 0.010, sulphur to 0.008 and nitrogen to 0.010. Properties depend on hitting those limits and on a melt practice that keeps impurities and segregation down. Aluminium is the hardening element and forms the precipitates that produce the strength of the aged conditions.

Melting

Material to AMS 5629 is normally double melted, vacuum induction melting followed by consumable-electrode vacuum arc remelting. The melt shop here runs a 3 t vacuum induction furnace, a 6 t vacuum arc remelting furnace and 3 t and 6 t protective-atmosphere electroslag furnaces, so that route runs in house instead of being bought in. For industrial work where a remelted ingot is not required, the electric arc furnace, ladle furnace and vacuum oxygen decarburisation route is used, with a 60 t maximum heat. State the specification and the melt route on the enquiry, because it decides which ingot gets scheduled and it moves the price.

04

Mechanical properties, H950 to H1150

Specified room-temperature minima, longitudinal, AMS 5629 and ASTM A564 Grade XM13 basis
Condition 0.2 % proof stress Tensile strength Elongation Reduction of area Hardness
A, solution treatednot specifiednot specified——363 HB max
H9501413 MPa / 205 ksi1517 MPa / 220 ksi10 %45 %45 HRC
H10001310 MPa / 190 ksi1413 MPa / 205 ksi10 %50 %43 HRC
H10251207 MPa / 175 ksi1276 MPa / 185 ksi11 %50 %41 HRC
H10501138 MPa / 165 ksi1207 MPa / 175 ksi12 %50 %40 HRC
H1100931 MPa / 135 ksi1034 MPa / 150 ksi14 %50 %34 HRC
H1150621 MPa / 90 ksi931 MPa / 135 ksi14 %50 %30 HRC

Published typical values sit above these minima. Typical longitudinal H1000 properties run near 1413 MPa proof stress and 1482 MPa tensile strength at 13 percent elongation and 45 HRC. Charpy V-notch impact energy climbs with ageing temperature, from roughly 27 J in H950 to about 103 J in H1150 and about 163 J in the overaged H1150M condition. Transverse typical values stay close to longitudinal, which is the practical reason the grade gets specified for thick forged sections. Acceptance is always against the minima of the ordered specification, and those are the figures reported on the certificate.

Physical data

Published physical properties, for guidance in design
Density, H10007.76 g/cm³ · 0.280 lb/in³
Modulus of elasticity, H1000195 GPa · 28.3 × 10³ ksi
Thermal conductivity at 100 °C14.0 W/m·K
Mean thermal expansion, 21 to 316 °C11.2 × 10⁻⁶ /K
Magnetic responseFerromagnetic in all conditions
Oxidation resistanceGood to about 593 °C (1100 °F)
05

Forging and heat treatment

The grade forges, hot heads and upsets without difficulty. The two rules that matter are the finishing temperature and the solution treatment.

Stock is heated uniformly to 1175 to 1205 °C (2150 to 2200 °F) and held about one hour at temperature. Forging stops above 955 °C (1750 °F). The piece is then air cooled to about 16 °C (60 °F), which is what sets the grain size. Every hot-worked piece is solution treated before ageing. Skip that and the part will not respond properly to the ageing treatment, whatever the furnace chart says.

Heat treatment conditions, ageing is four hours at temperature followed by air cooling
ConditionTreatmentNotes
A925 °C ± 8 °C, cool below 16 °CSolution treated, fully transformed to martensite. Sections under about 230 cm² may be liquid quenched, heavier sections air cooled
H950510 °C, 4 h, air coolHighest strength and hardness, slowest machining
H1000538 °C, 4 h, air coolLowest ageing temperature suggested where stress-corrosion cracking governs
H1025552 °C, 4 h, air coolBalance of strength and toughness
H1050566 °C, 4 h, air coolCommon on valve and pump parts
H1100593 °C, 4 h, air coolHigher toughness, easier machining
H1150621 °C, 4 h, air coolOveraged. Will not respond to further ageing without a fresh solution treatment
RH950Cold treat to −73 °C for 2 h within 24 h of solution treatment, warm to room temperature, then 510 °C, 4 h, air coolHighest typical strength level
H1150M760 °C, 2 h, air cool, then 621 °C, 4 h, air coolBest machinability. Needs re-solution treatment to reach higher strengths

Ageing contracts the part by a predictable amount, roughly 0.0004 to 0.0006 in/in for H950 and H1000, 0.0005 to 0.0008 for H1050 and 0.0008 to 0.0012 for H1100. We allow for it when pre-machining anything that gets aged after machining. One more thing worth knowing on incoming inspection: the hardness range of H1150 overlaps the solution-treated range, so a hardness reading alone cannot prove which condition a part is in. The heat treatment record on the certificate is the only evidence.

06

Machining, welding and corrosion

The grade machines in the solution-treated condition and in the aged conditions. In condition A, tool life and finish are good at surface speeds roughly 20 to 30 percent below those used on 17Cr-4Ni and on Types 302 and 304. Machinability in the aged conditions improves as the ageing temperature rises, and H1150M is the easiest of them. At 45 HRC minimum, H950 turning, drilling and milling is slow and hard on tooling, so the usual sequence is rough machine in condition A, age, then finish. Bar and forging stock is cold sawn rather than abrasive cut, because abrasive wheel cutting can leave fine surface cracks behind.

Welding runs by inert-gas shielded or resistance processes. Matching 13-8 filler is used where the weld has to match the base metal, and an austenitic filler such as E/ER308L where it does not. Welding in the solution-annealed condition is normally satisfactory, and the best combination of strength, ductility and corrosion resistance comes from solution treating the welded part and then ageing it.

On corrosion, the H950 condition resists rusting in 5 percent salt fog about as well as Type 304, and general resistance in strongly oxidising and reducing acids and in atmospheric exposure approaches Type 304. Resistance is highest fully hardened and falls slightly as ageing temperature rises, while resistance to stress-corrosion cracking moves the other way and improves with ageing temperature. That is the whole reason for the 538 °C minimum recommendation. Finished parts go out free of scale and embedded iron, and passivated.

07

Where the grade is used

Published applications cluster in high-duty service where strength and corrosion resistance are both required: valve parts and fittings, cold-headed and machined fasteners, shafts and pins, landing gear components, lockwashers, aerospace parts, nuclear reactor components, injection moulding equipment, and petrochemical duty that needs resistance to stress-corrosion cracking.

In our own order book this grade leaves mostly as valve stems, seat rings and bodies for ball, gate, globe and check valves, as pump and compressor shafts and sleeves, and as forged rings and discs for rotating equipment. If the enquiry is for a large pressure-boundary component, we will usually suggest pricing 17-4 PH or 15-5 PH alongside it before committing, because 13-8 costs more and the extra toughness is not always being used.

08

Inspection and certification

Ultrasonic examination follows the standard named on the order, EN 10228-3, SEP 1921 or ASTM A388, to the acceptance class stated on the purchase order. Chemical analysis, tensile test, hardness and, where required, Charpy V-notch impact test are reported on an inspection certificate to EN 10204 type 3.1, or type 3.2 counter-signed by a third party such as SGS, BV, TUV or Lloyd's Register. Dimensional reports, positive material identification, liquid penetrant examination, grain size and intergranular corrosion testing are added on request. Heat-number traceability runs from the melt to the shipped part, and the works holds CCS, BV, DNV, LR and NK approvals.

09

Requesting a quotation

Send a drawing as PDF, DWG or STEP, or the finished dimensions. State the grade and specification, for example UNS S13800 forged ring to ASTM A705 condition H1050, then the quantity, the delivery condition, the melt route if it is specified, the testing and certificate requirements, and the destination port. We reply with forging weight, machining allowance, price and lead time. Minimum order is 10 kg with no minimum piece count, and normal lead time is 20 to 60 days.

10

Questions we are asked about this grade

Is UNS S13800 the same as PH13-8Mo?

Yes. UNS S13800 is the unified numbering designation for the alloy sold as PH 13-8 Mo, and the same material appears as 13-8 PH, alloy 13-8, ASTM grade XM-13, EN 1.4534 and X3CrNiMoAl13-8-2. PH 13-8 Mo is a registered trademark of Armco Inc., so a certificate normally carries the generic designations.

Which specification goes on a forging order?

ASTM A705 or ASME SA705, grade XM-13, with the condition required. Bar and machined-from-bar parts go to ASTM A564 or ASME SA564 Grade XM13, and aerospace work to AMS 5629. ASTM B564 is for nickel-alloy forgings and should not be used here.

What are the H950 properties?

Minimum 1413 MPa (205 ksi) 0.2 percent proof stress, 1517 MPa (220 ksi) tensile strength, 10 percent elongation, 45 percent reduction of area and 45 HRC.

Which aged condition should be specified?

H950 for maximum strength and hardness, accepting the lowest toughness and the hardest machining. H1000 and above trade strength for toughness and for resistance to stress-corrosion cracking, with 538 °C the suggested minimum ageing temperature where cracking is the governing risk. H1150 and H1150M are overaged conditions for forming and machining, and both need re-solution treatment before further ageing.

Can you ship in the solution-treated condition for us to age?

Yes. Condition A so that you machine and age, or solution treatment and ageing done here with the final properties certified. Decide at enquiry stage, because it changes the machining allowance and the contraction we have to allow for.

Can you supply double-melted material to AMS 5629?

Yes. Vacuum induction melting at 3 t, vacuum arc remelting at 6 t and protective-atmosphere electroslag at 3 t and 6 t all run in this works, so a double-melted ingot does not have to be subcontracted. Name the melt route on the enquiry.

What size can you forge?

Rings up to 6,000 mm outside diameter on the radial-axial mill, down to 50 mm by upsetting and punching. Shafts up to 14,000 mm turned length. Discs, tube sheets and blocks up to 5,000 mm machined diameter. Bored cylinders up to 1,600 mm diameter by 10,000 mm. Single-piece weight up to 30,000 kg.

Is UNS S13800 magnetic?

Yes. It is martensitic and ferromagnetic in both the solution-treated and aged conditions, so it cannot be used where a non-magnetic grade is required.

11

Data basis

Composition, property, forging and heat treatment data on this page follow the published requirements of AMS 5629, ASTM A564 and ASME SA564 Grade XM13, ASTM A705 and ASME SA705, together with mill and distributor data sheets for alloy 13-8. Figures are given for design and enquiry work. The governing values for any order are those of the specification and revision written on the purchase order, as reported on the EN 10204 certificate. Plain-text version of this page: UNS-S13800.md.