904S13 Forgings (904L, UNS N08904, EN 1.4539)
Seamless rolled rings, flanges, shafts, discs, sleeves, bushings, tube sheets and bars forged to drawing in 904S13 by Jiangyin Jiangnan Metal Co., Ltd.
904S13 is the British Standard designation for the super-austenitic stainless steel sold internationally as 904L, UNS N08904 and EN 1.4539 (X1NiCrMoCu25-20-5). The composition runs about 20 percent chromium, 25 percent nickel, 4 to 5 percent molybdenum and 1 to 2 percent copper on a low-carbon base. Copper is what sets the grade apart from 316L and 317L: it gives useful service in reducing acids such as sulphuric and phosphoric, while the high nickel content handles chloride stress corrosion cracking. PREN is about 35. The alloy is non-magnetic and is supplied solution annealed.
Forged, the grade goes into rolled rings, flanges, valve bodies, pump shafts, tube sheets and discs for acid plant, seawater and desalination duty, flue gas scrubbers, and pulp bleaching lines. We forge it at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, with ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388 and certification to EN 10204 3.1 or 3.2.
- UNS
- N08904
- EN number
- 1.4539
- BS
- 904S13
- Structure
- Austenitic
- PREN
- approx. 35
- Max service
- approx. 400 °C
Grade description
904S13 sits between standard 316L and the 6 percent molybdenum super-austenitics in corrosion performance. It is non-stabilised and low in carbon, so it resists intergranular attack both as delivered and in the sensitised condition, and it combines that with pitting and crevice resistance and good weldability. Along with sulphuric and phosphoric acid it tolerates formic, acetic, oxalic, citric and lactic acids, concentrated salt solutions, nitrates, chlorides, hydrogen sulphide, hydrogen chloride, seawater, acetates and sulphates.
Two limits matter when specifying it. First, temperature: oxidation resistance is good but structural stability collapses above roughly 400 °C, so the grade has no place in sustained hot service. Second, nitric acid: because 904S13 carries molybdenum it is less resistant to nitric acid than the molybdenum-free grades 304L and 310L. Its strength is in reducing media, not oxidising ones.
Equivalent designations
| Standard | Designation |
|---|---|
| BS (old British) | 904S13 |
| UNS / ASTM | N08904, 904L. Forgings to ASTM A182 Grade F904L, flat product to ASTM B625 |
| EN / DIN | 1.4539, X1NiCrMoCu25-20-5 |
| AFNOR | Z2NCDU25-20 |
| JIS | SUS 890L; tube and pipe as SUS 317J5L TK / TP |
| Swedish SS | 2562 |
| Polish PN | 0H22N24M4TCu |
Chemical composition
BS 904S13 and UNS N08904 are close but not interchangeable on paper. The British window is tighter on chromium and nickel and allows slightly more carbon. Order against whichever specification the drawing calls out.
| Element | UNS N08904 | BS 904S13 | EN 1.4539 |
|---|---|---|---|
| Carbon | 0.02 max | 0.03 max | 0.02 max |
| Chromium | 19.00–23.00 | 19.0–22.0 | 19.0–21.0 |
| Nickel | 23.00–28.00 | 24.0–27.0 | 24.0–26.0 |
| Molybdenum | 4.00–5.00 | 4.0–5.0 | 4.0–5.0 |
| Copper | 1.00–2.00 | 1.0–2.0 | 1.2–2.0 |
| Manganese | 2.00 max | 2.0 max | 2.0 max |
| Silicon | 1.00 max | 1.0 max | 0.7 max |
| Phosphorus | 0.045 max | 0.040 max | 0.030 max |
| Sulphur | 0.035 max | 0.025 max | 0.010 max |
| Nitrogen | 0.10 max (ASTM A182 F904L) | – | 0.15 max |
| Iron | Balance | ||
Mechanical properties
For a forging order the governing figures are the ASTM A182 F904L minima. The ASTM B625 flat-product values are shown alongside because they are the numbers most general 904L literature quotes.
| Property | ASTM A182 F904L, forgings | ASTM B625, flat product |
|---|---|---|
| Tensile strength | 490 MPa (71 ksi) min | 490 MPa min |
| Yield strength, 0.2 percent | 215 MPa (31 ksi) min | 220 MPa min |
| Elongation | 35 percent min in 50 mm or 4D | 36 percent min in 50 mm |
| Hardness | not specified | about 150 HB, 70–90 HRB typical |
European product forms
Bar above 63 mm to EN 10088-5 runs 530 to 730 MPa tensile with yield above 230 MPa and elongation above 35 percent; bar 16 to 63 mm runs 530 to 880 MPa against the same yield floor. Seamless tube to EN 10216-5 in the +AT condition is 520 to 720 MPa, with longitudinal impact energy above 120 J at 20 °C and transverse impact energy above 60 J at minus 196 °C. That cryogenic toughness is one of the less advertised advantages of the grade.
Proof stress at temperature
| Temperature, °C | 100 | 200 | 300 | 400 | 500 |
|---|---|---|---|---|---|
| Rp0.2, MPa min | 205 | 175 | 145 | 125 | 110 |
| Modulus E, GPa | 190 | 182 | 174 | 166 | 158 |
Values above 400 °C are given for completeness only. Sustained service at those temperatures is not recommended for this grade.
Physical properties
| Property | Value |
|---|---|
| Density | 7 900 kg/m³; mill datasheets also quote 7.95 g/cm³ |
| Melting range | 1 300–1 390 °C |
| Modulus of elasticity, 20 °C | 190–195 GPa depending on source |
| Thermal conductivity, 20 °C | 11.5–12 W/m·K |
| Mean thermal expansion, 0–100 °C | 15–15.8 ×10-6/K, rising to 17.3 ×10-6/K at 500 °C |
| Specific heat, 0–100 °C | 450–500 J/kg·K |
| Electrical resistivity | 952 nΩ·m |
| Magnetic response | Non-magnetic in the annealed condition |
Where published datasheets differ slightly, both figures are given rather than averaged. Use the value from the specification your drawing invokes.
Corrosion performance and grade selection
Resistance to warm seawater and chloride attack is one of the reasons the grade is specified offshore. High nickel underpins the stress corrosion cracking resistance, copper the behaviour in reducing acids. After cold work the material should be re-solution treated to restore full stress corrosion resistance in demanding environments.
| Alloy | UNS | PREN |
|---|---|---|
| 316 | S31600 | 27 |
| Alloy 20 | N08020 | 28 |
| Incoloy 825 | N08825 | 31 |
| 904S13 / 904L | N08904 | 35 |
| Duplex 2205 | S31803 | 36 |
| 254 SMO | S31254 | 43 |
| Super duplex 2507 | S32750 | 43 |
PREN = %Cr + 3.3 × %Mo + 16 × %N. A PREN of 32 or more is the common benchmark for seawater pitting resistance, which places 904S13 above the line but not far above it.
| Alternative | Trade-off against 904S13 |
|---|---|
| 316L | Lower cost, much lower corrosion resistance. |
| 6 percent Mo super-austenitic | Specify when higher pitting and crevice resistance is required. |
| Duplex 2205 | Similar corrosion resistance with higher strength at lower cost, but not suitable above about 300 °C and lower in ductility. |
| Super duplex | Specify when both higher corrosion resistance and higher strength are needed. |
Cost drives most substitutions. 904S13 carries expensive nickel and molybdenum, and a good share of the work that once went to this grade now goes to duplex 2205. Where an austenitic structure is genuinely required, or where the service temperature rules duplex out, 904S13 remains the answer.
Forging, heat treatment and fabrication
Hot working covers roughly 900 to 1200 °C. Finishing below about 950 °C invites cracking, and some mill practice narrows the window to 1150 down to 950 °C. Solution annealing follows at about 1050 to 1150 °C with rapid cooling; wider windows up to 1175 °C are also published. Being austenitic, the grade takes its strength from cold work, not from heat treatment, and annealing exists to restore the soft, fully corrosion-resistant condition.
In our shop, billet is upset and drawn on hydraulic open-die presses, ring blanks are pierced and rolled on a radial-axial ring mill, and every piece is solution annealed and quenched before machining allowance is set. The alloy is low in sulphur, so it machines by conventional methods and cold bends to a small radius. Subsequent annealing after bending is usually unnecessary unless the part will face severe stress corrosion conditions.
Welding can be done by all conventional processes with no preheat and no post-weld heat treatment. Matching 904L electrodes and rods are used, per AS 1554.6. Heavily restrained weldments can suffer hot cracking, so joint design and restraint deserve attention.
Forged products in 904S13
Everything is made to drawing; there is no fixed catalogue. Send a drawing, a dimensioned sketch, or simply outside diameter, inside diameter, height and quantity.
| Form | Typical use |
|---|---|
| Seamless rolled rings | Pump and valve bodies, bearing races, flanged connections in acid and seawater duty. See the rolled ring page. |
| Forged flanges | Weld neck, slip-on, blind and threaded, usually to ASTM A182 F904L with ASME B16.5 dimensions. |
| Shafts and spindles | Seawater pumps, agitators, scrubber shafts, gearbox and transmission shafts. |
| Discs, blanks and hubs | Blind covers, valve discs, closure heads, gear blanks. |
| Tube sheets | Heat exchangers and condensers in seawater-cooled and acid service. |
| Sleeves, bushings and cylinders | Pump wear parts, liners, sleeves for down-hole and process equipment. |
| Bars, blocks and step shafts | Machining stock for valve stems, seats, bodies and manifolds. |
| Hollow bar and nozzles | Nozzles, weldolets and heavy-wall sections for pressure vessels. |
Testing and documentation
Ultrasonic testing is carried out to EN 10228-3, SEP 1921 or ASTM A388 as the order requires. Forgings ship with an EN 10204 3.1 inspection certificate, or a 3.2 certificate counter-signed by a third party such as SGS, BV or TUV. Chemical analysis, tensile and impact results, heat treatment records and heat traceability are included. Positive material identification and dimensional reports are available on request.
Applications
Acid service is the core market: plant handling sulphuric, phosphoric and acetic acid, oil refinery components, seawater cooling systems, gas scrubbing plant, electrostatic precipitator wiring, and pulp and paper processing. The grade also goes into desalination systems, condensers and seawater-cooled heat exchangers, scrubbers in coal-fired power stations, exhaust filtration, shipbuilding and offshore pipework, and food, cryogenic and pharmaceutical equipment.
In forged form that means seawater ballast and cooling pump parts, gate and ball valve bodies and stems for chloride service, exchanger tube sheets and channel flanges, scrubber shafts and rings, wellhead and down-hole components in sour and chloride-bearing fluids, and crystalliser and reactor internals in fertiliser and fine chemical plant.
Request a quotation
Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory, No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Send a drawing or the main dimensions and we will come back with price, forged weight, lead time and the test plan.
sales@steelforgepieces.com 0086-189-2135-9659 Contact page
Useful to include: specification called out on the drawing (904S13, 904L, UNS N08904, EN 1.4539 or ASTM A182 F904L), rough or finished dimensions, quantity, delivery condition, NDT requirement and certificate type.
Questions we are asked most
Is 904S13 the same as 904L?
Same alloy, different national standard, slightly different limits. BS 904S13 permits carbon to 0.03 percent with chromium 19.0 to 22.0 and nickel 24.0 to 27.0. UNS N08904 permits carbon to 0.02 percent with the wider chromium 19.00 to 23.00 and nickel 23.00 to 28.00. Buy against the specification named on the drawing.
What are the mechanical minima for forgings?
ASTM A182 Grade F904L calls for 490 MPa (71 ksi) tensile minimum, 215 MPa (31 ksi) yield minimum and 35 percent elongation in 50 mm or 4D. Flat product to ASTM B625 is quoted at 490 and 220 MPa with 36 percent elongation and about 150 HB.
Is 904S13 suitable for seawater?
PREN of about 35 clears the usual seawater benchmark of 32, though not by a wide margin. For hot, stagnant or crevice-prone seawater, super duplex 2507 or 254 SMO at around 43 are the more conservative choices.
What forging and annealing temperatures apply?
Forge and ring-roll between roughly 900 and 1200 °C, and avoid finishing below about 950 °C. Solution anneal at about 1050 to 1150 °C and cool rapidly. Wider annealing windows up to 1175 °C are published by some sources.
How hot can it run?
About 400 °C. Oxidation resistance is good, but structural stability drops away above that, so the grade is not intended for sustained hot service. For that, move to a nickel-base alloy.
How does it behave in nitric acid?
Worse than its overall reputation suggests. Because it is molybdenum-bearing it is less resistant to nitric acid than molybdenum-free 304L and 310L. Its advantage is in reducing acids.
Can it be welded?
Yes, by all conventional processes, with no preheat and no post-weld heat treatment. Matching 904L consumables are used. Heavily restrained weldments can hot crack, and cold-worked material should be re-solution treated where stress corrosion conditions are severe.
Do you take one-off pieces?
Open-die forging is a single-piece process, so prototypes and one-offs are quoted alongside production batches. Email sales@steelforgepieces.com or call 0086-189-2135-9659 with the drawing.
Related grades
Other stainless grades we forge: A286, AISI 330, 17-4PH, 15-5PH, 17-7PH and PH13-8Mo. Where 904S13 is not enough, buyers commonly step up to Alloy 31, Incoloy 825, Incoloy 926, Hastelloy C-276 or Inconel 625.
Data on this page is compiled from published grade datasheets for 904L, UNS N08904 and EN 1.4539, and from ASTM A182 F904L and ASTM B625 requirements. Last reviewed 29 September 2026 by the engineering team at Jiangyin Jiangnan Metal Co., Ltd. Verify all design values against the governing specification for your project.