1.4568 Forgings: X7CrNiAl17-7 / 17-7 PH Precipitation-Hardening Stainless Steel
EN 1.4568X7CrNiAl17-717-7 PHUNS S17700AISI 631SUS 631
1.4568 is the EN material number for X7CrNiAl17-7, a semi-austenitic precipitation-hardening chromium-nickel-aluminium stainless steel sold commercially as 17-7 PH and listed as UNS S17700 and AISI 631. The grade contains 16.0 to 18.0 % chromium, 6.5 to 7.8 % nickel and 0.7 to 1.5 % aluminium. Tensile strength runs from 896 MPa in the annealed Condition A to 1828 MPa in Condition CH 900.
Jiangyin Jiangnan Metal Co., Ltd. is an open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. The factory forges 1.4568 into seamless rolled rings, forged rings, flanges, shafts, discs, sleeves, bushings, tube sheets, hollow bars and round bars, working to customer drawing from EAF+VOD or ESR-remelted stock, with EN 10204 3.1 or 3.2 certification. For quotations contact sales@steelforgepieces.com or 0086-189-2135-9659.
- EN number
- 1.4568
- EN name
- X7CrNiAl17-7
- UNS / AISI
- S17700 / 631
- Alloy family
- Semi-austenitic PH stainless
- Density
- 7.81 g/cm³
- Peak tensile
- 1828 MPa (CH 900)
- Max service temp.
- 480 °C (900 °F)
- Certification
- EN 10204 3.1 / 3.2
What is 1.4568 stainless steel?
1.4568 is a precipitation-hardening stainless steel standardised in EN 10088 under the chemical designation X7CrNiAl17-7. The grade is semi-austenitic. In the solution-annealed state it is austenitic, weakly magnetic, ductile and easy to machine or form. Strength comes in a second stage: the austenite is conditioned so that it transforms to martensite, then aged to precipitate nickel-aluminium intermetallics.
Parts are therefore machined or formed soft and hardened afterwards. Dimensional change through the hardening cycle stays under about 0.1 %, well below the movement produced by a quench-and-temper cycle. Close-tolerance rings, spring elements, diaphragms, valve internals and fasteners are the common applications.
The hardening element is aluminium, not copper. This separates 1.4568 from 17-4 PH (1.4542), where copper does the work. The H900, H1025 and H1150 condition names belong to 17-4 PH and do not apply to 1.4568. Conditions for 1.4568 are A, T, R 100, TH 1050, RH 950, C and CH 900.
1.4568 equivalent grades and cross reference
| Standard / system | Designation | Notes |
|---|---|---|
| EN (number) | 1.4568 | EN 10088-1/-2/-3, EN 10151, EN 10270-3 |
| EN (name) | X7CrNiAl17-7 | Chemical designation |
| Trade name | 17-7 PH | Original Armco designation |
| UNS | S17700 | USA unified numbering |
| AISI / SAE | 631 | Type 631 |
| ASTM | A693 Gr. 631, A564 Type 631, A579 Gr. 62 | Sheet/strip, bar/shape, forgings |
| AMS | AMS 5528, 5529, 5568, 5644 | 5644 covers bars, forgings and rings |
| JIS (Japan) | SUS 631 | JIS G 4303 / G 4313 |
| GB (China) | 07Cr17Ni7Al (formerly 0Cr17Ni7Al) | GB/T 1220, GB/T 4238 |
| AFNOR (France) | Z8CNA17-7 | NF A35-575 |
| BS (UK) | 301S81 | Closest equivalent |
| ISO | X7CrNiAl17-7 | ISO 15510 |
Cross-reference table for guidance. Equivalent grades are closest-known matches, not exact substitutes. Confirm the governing specification on the drawing before ordering.
Chemical composition of 1.4568
The chemical composition of 1.4568 / X7CrNiAl17-7 to EN 10088-3 is given below, in weight percent.
| Limit | C | Si | Mn | P | S | Cr | Ni | Al | Fe |
|---|---|---|---|---|---|---|---|---|---|
| Min | – | – | – | – | – | 16.00 | 6.50 | 0.70 | Bal. |
| Max | 0.09 | 0.70 | 1.00 | 0.040 | 0.015 | 18.00 | 7.80 | 1.50 | Bal. |
Source: EN 10088-3, stainless steel bars, rods, wire, sections and bright products. Where a customer specifies UNS S17700 to ASTM A564 or A693, the American limits differ: Mn 1.00 max, Si 1.00 max, S 0.030 max and Ni 6.50 to 7.75 %. Jiangyin Jiangnan Metal Co., Ltd. melts to whichever specification the order calls out.
Melting practice
1.4568 for forging is melted by EAF + VOD, electric arc furnace with vacuum oxygen decarburisation, as standard. Where cleanliness, transverse ductility or aerospace inclusion ratings are required, the grade is supplied ESR, electroslag remelted. The aluminium content makes the alloy sensitive to melt-shop practice. Aluminium loss during remelt shifts the ageing response, so heat chemistry is verified on the finished forging as well as on the ingot.
1.4568 heat treatment conditions
1.4568 is supplied and used in defined conditions. Each condition is a complete route, not a single temperature. The table below gives the standard cycles.
| Condition | Route | Purpose |
|---|---|---|
| A | Solution anneal 1065 °C (1950 °F), air cool | Soft, austenitic, formable and machinable. Standard as-delivered condition for forgings. |
| T | From A: 760 °C (1400 °F) / 90 min, cool to 15 °C (60 °F) within 1 h | Austenite-conditioned, martensitic, not yet aged. Intermediate stage. |
| TH 1050 | From T: age 565 °C (1050 °F) / 90 min, air cool | High strength with good toughness and stable dimensions. Most common hardened condition for forgings. |
| R 100 | From A: 955 °C (1750 °F) / 10 min, air cool, then −73 °C (−100 °F) / 8 h | Sub-zero conditioned, martensitic, not yet aged. Intermediate stage. |
| RH 950 | From R 100: age 510 °C (950 °F) / 60 min, air cool | Highest strength obtainable from annealed stock. 1620 MPa, 48 HRC. |
| C | Cold reduced 60 % | Strain-hardened strip and wire. Not applicable to heavy forgings. |
| CH 900 | From C: age 480 °C (900 °F) / 60 min, air cool | Peak strength 1828 MPa. Thin cold-worked sections only. |
Times are soak-at-temperature. Heavy forged sections need soak time extended by section thickness. Cycles follow the alloy producer's published practice and AMS 2759/3.
Which condition should be specified for a forging?
- Condition A: order here if the part will be machined in-house. Most 1.4568 rings, bars and discs leave the factory this way.
- TH 1050: the working default for hardened heavy sections. It tolerates section-size variation better than RH 950 and gives a better toughness-to-strength balance.
- RH 950: specify when maximum strength is required and the part can accept the sub-zero cycle and lower ductility, around 6 % elongation.
- CH 900: cold-worked product only. It cannot be reached in a heavy open-die forging.
1.4568 responds sharply to small chemistry and time-at-temperature variations. Jiangyin Jiangnan Metal Co., Ltd. runs a sacrificial test coupon from the same heat and the same furnace charge as the forging, and reports its results on the EN 10204 certificate.
Mechanical properties of 1.4568
| Property | Condition A | Condition TH 1050 | Condition RH 950 | Condition C | Condition CH 900 |
|---|---|---|---|---|---|
| Tensile strength, MPa (ksi) | 896 (130) | 1379 (200) | 1620 (235) | 1517 (220) | 1828 (265) |
| 0.2 % proof strength, MPa (ksi) | 276 (40) | 1276 (185) | 1517 (220) | 1310 (190) | 1793 (260) |
| Elongation in 50 mm (2 in.), % | 35 | 9 | 6 | 5 | 2 |
| Hardness, Rockwell | 85 HRB | 43 HRC | 48 HRC | 43 HRC | 49 HRC |
Typical values for guidance, measured on thin sections. Heavy forged sections normally land at the lower end of the range, because cooling rate and ageing response vary through thickness. Acceptance minima, test location (surface, mid-radius or centre) and test direction (longitudinal, transverse or tangential) should be agreed on the drawing or purchase specification before order.
Physical properties of 1.4568
| Property | Value (metric) | Value (imperial) |
|---|---|---|
| Density | 7.81 g/cm³ | 0.282 lb/in³ |
| Melting range | 1400 to 1440 °C | 2550 to 2620 °F |
| Modulus of elasticity (Condition A) | 200 GPa | 29 × 10&sup6; psi |
| Modulus of elasticity (TH 1050) | 204 GPa | 29.5 × 10&sup6; psi |
| Mean coeff. of thermal expansion, 20 to 100 °C | 11.6 µm/m·°C | 6.4 µin/in·°F |
| Thermal conductivity at 100 °C | 16.4 W/m·K | 9.5 Btu/h·ft·°F |
| Specific heat, 0 to 100 °C | 460 J/kg·K | 0.11 Btu/lb·°F |
| Electrical resistivity | 0.83 µΩ·m | 500 Ω·circ mil/ft |
| Magnetic response | Weakly magnetic in Condition A, ferromagnetic after conditioning and ageing | |
| Max. continuous service temperature | 480 °C | 900 °F |
Corrosion resistance
General corrosion resistance of 1.4568 is close to austenitic type 301 / 1.4310. It is better than the 400-series martensitic stainless steels, below 304 and well below 316. The grade resists atmospheric exposure, fresh water, mild chemical environments and many petrochemical process streams. It contains no molybdenum, so it is not a chloride-pitting grade. For seawater, brine or sour service, specify a duplex, super-duplex or nickel-alloy forging such as Incoloy 825. Fully aged high-strength conditions are more susceptible to stress-corrosion cracking than Condition A, and TH 1050 is preferred over RH 950 where SCC risk exists.
1.4568 forged products and size capability
Jiangyin Jiangnan Metal Co., Ltd. produces the following 1.4568 open-die forgings to customer drawing or finished dimensions.
- Rings: seamless rolled rings, forged rings, retaining rings, valve seat rings, bearing rings, slewing-ring blanks
- Flanges: forged flanges, weld-neck, slip-on, blind and custom-profile flange blanks
- Bars: forged round bars, hollow bars, square bars, rectangular blocks, step shafts
- Shafts: forged shafts, spindles, eccentric shafts, crankshafts, pump shafts, drive shafts
- Discs: forged discs, disks, blanks for gears, turbine and impeller blanks
- Hollow sections: forged tubes, forged pipes, sleeves, bushings, cylinders, nozzles
- Plate-type: tube sheets, forged blocks, valve bodies, manifolds
| Product form | Size range | Unit weight |
|---|---|---|
| Seamless rolled rings | OD 150 to 3000 mm, height up to 1000 mm | 10 to 8000 kg |
| Forged round bars | Dia. 60 to 800 mm, length up to 6000 mm | 20 to 6000 kg |
| Forged discs / blanks | Dia. 150 to 2500 mm, thickness 30 to 600 mm | 20 to 8000 kg |
| Forged shafts | Dia. 80 to 900 mm, length up to 8000 mm | 50 to 10000 kg |
| Sleeves / bushings / hollow bars | OD 120 to 1500 mm, ID from 60 mm | 10 to 5000 kg |
| Flanges / tube sheets | OD up to 3000 mm | 20 to 8000 kg |
Single-piece and prototype quantities accepted. Open-die forging needs no dedicated die. Lead time is 25 to 45 days depending on section size, heat-treatment condition and testing scope.
Manufacturing route and quality control
- Melting. EAF + VOD as standard. ESR remelt where cleanliness or aerospace inclusion ratings are specified.
- Forging. Open-die forging with a controlled forging ratio, minimum 3:1 on heavy sections and higher where transverse properties are specified, to break down the as-cast structure and close centreline porosity.
- Ring rolling. Seamless radial-axial rolling for ring product, giving continuous circumferential grain flow that a cut-and-welded ring cannot match.
- Heat treatment. Solution anneal to Condition A. TH 1050 and RH 950 cycles on request, with charge-attached test coupons and recorded furnace charts.
- Machining. Rough, semi-finish or finish machining to drawing, including CNC turning, boring and milling.
- Non-destructive testing. Ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388. Liquid penetrant to ASTM E165 or EN ISO 3452. Magnetic particle where the condition permits.
- Destructive and chemical testing. Spectrographic chemical analysis, tensile, hardness, impact, intergranular corrosion testing to ASTM A262 where specified, and grain-size assessment.
- Certification. EN 10204 3.1 as standard. EN 10204 3.2 witnessed by TUV, BV, SGS, DNV or Lloyd's Register on request.
Applications of 1.4568 forgings
Pumps, compressors and rotating equipment
1.4568 seamless rolled rings and forged shafts run in chemical pumps, plunger pumps, industrial air compressors, power generators, nitrogen generators, gas compressors, turbines and gear boxes. High fatigue strength combined with dimensional stability through hardening is what puts the grade into these parts.
Pressure equipment and heat transfer
1.4568 forged tube sheets, forged flanges, forged pipes and forged tubes are specified for pressure vessels, air receivers, shell-and-tube heat exchangers, columns, towers, tanks, silos, preheaters and process modules operating below the 480 °C service limit.
Valves and flow control
1.4568 forged valve stems, valve seat rings, valve blocks and valve bodies go into ball valves, check valves, globe valves, gate valves, plug valves and strainers. Aged material resists galling and seat wear at high seating loads.
Oil, gas and offshore
1.4568 forged bushings, sleeves, discs and rings serve subsea and deepwater offshore oil production systems, wellhead and Christmas-tree components and processing units. The corrosion note above applies: the grade is not suitable for direct chloride or sour service.
Springs, diaphragms and precision elements
1.4568 can be formed soft and then hardened with very little distortion, which makes it the standard grade for Belleville washers, spiral-wound gasket windings, diaphragms, bellows, retaining rings and precision spring elements.
Heavy industry
1.4568 forged rolls, wheels, manifolds, nozzles and crankshafts are used in cement mills, sugar mills, concrete mixers, shipbuilding, heavy machinery, pulp and paper plant, and pharmaceutical and biochemical equipment.
Machining, welding and fabrication of 1.4568
Machining. Rough machine in Condition A, where machinability is close to austenitic grades 302, 303 and 304 and much easier than in the aged conditions. Leave a finishing allowance of 0.3 to 0.8 mm per side to absorb heat-treatment movement, then finish machine after ageing. In the RH 950 and CH 900 conditions the material reaches 48 to 49 HRC and turning, drilling, tapping and CNC milling become demanding. Use carbide or ceramic tooling, rigid setups, reduced surface speed, positive feed and generous coolant. Avoid interrupted cuts and small-diameter drilling in the aged condition where the design allows.
Welding. 1.4568 is welded by GTAW, GMAW, plasma and resistance methods, preferably in Condition A and preferably without filler where joint design permits. Where filler is required, use 17-7 PH filler so that the weld responds to the same ageing cycle. Austenitic fillers such as 308 or 309 give a weld that will not harden with the parent metal. Solution anneal the complete assembly and then take it through the chosen condition so that weld and parent metal age together. Welding in the fully aged condition is not recommended, because the heat-affected zone over-ages and loses strength locally.
Forming. Condition A material forms and bends readily but work-hardens quickly, so intermediate annealing may be needed for severe forming. The material sits close to its final dimensions after ageing, with dimensional change through the TH 1050 cycle typically under 0.1 %.
1.4568 frequently asked questions
What is 1.4568 stainless steel?
1.4568 is the EN material number for X7CrNiAl17-7, a semi-austenitic precipitation-hardening chromium-nickel-aluminium stainless steel. It is the European designation of the alloy sold as 17-7 PH, and it corresponds to UNS S17700 and AISI 631. The grade contains 16.0 to 18.0 % chromium, 6.5 to 7.8 % nickel and 0.7 to 1.5 % aluminium. Strength is developed by austenite conditioning followed by ageing, not by a quench.
Is 1.4568 the same as 17-7 PH?
Yes, the same alloy under different designation systems. 1.4568 and X7CrNiAl17-7 are the European EN 10088 designations. 17-7 PH is the original trade name. UNS S17700 is the American unified number and AISI 631 is the AISI type number. JIS calls the grade SUS 631 and the Chinese GB standard calls it 07Cr17Ni7Al.
What is the difference between 1.4568 (17-7 PH) and 17-4 PH?
17-4 PH (1.4542 / UNS S17400) is a martensitic PH stainless steel hardened by copper precipitation in H-conditions such as H900, H1025 and H1150. 1.4568 / 17-7 PH is semi-austenitic and hardened by aluminium. It is austenitic and formable in Condition A, then taken to strength through austenite conditioning and ageing in TH 1050, RH 950 or CH 900. The H900 and H1025 names do not apply to 1.4568. 17-7 PH gives higher peak strength and better spring and fatigue behaviour in thin sections. 17-4 PH is simpler to heat treat in heavy forged sections and is the usual choice for large valve bodies and pump shafts.
What heat treatment conditions are available for 1.4568 forgings?
Forgings are normally supplied in Condition A, solution annealed at about 1065 °C and air cooled, so the customer can machine before hardening. Jiangyin Jiangnan Metal Co., Ltd. also supplies forgings heat treated to Condition TH 1050 (austenite conditioning at 760 °C, cool to 15 °C, age at 565 °C), Condition RH 950 (conditioning at 955 °C, sub-zero cooling to −73 °C, age at 510 °C), and Condition CH 900 for cold-worked product. Full furnace charts and coupon test results accompany the certificate.
What tensile strength can 1.4568 reach?
Typical values: 896 MPa (130 ksi) in Condition A, 1379 MPa (200 ksi) in TH 1050, 1620 MPa (235 ksi) in RH 950 and up to 1828 MPa (265 ksi) in CH 900. Heavy forged sections usually achieve the lower end of the published range, so acceptance values, test location and test direction should be agreed on the drawing before order.
What forged shapes can be produced in 1.4568?
Jiangyin Jiangnan Metal Co., Ltd. produces 1.4568 as seamless rolled rings, forged rings, flanges, round bars, hollow bars, shafts, spindles, discs, disks, sleeves, bushings, tube sheets, forged pipes and tubes, valve bodies, valve seat rings, gear blanks and custom open-die forgings to drawing. Rings run from 150 mm to 3000 mm outside diameter, with single pieces up to about 10 tonnes.
What certification is supplied with 1.4568 forgings?
An EN 10204 3.1 inspection certificate is supplied as standard, covering chemical analysis, heat-treatment record, mechanical test results and dimensional report. EN 10204 3.2 certification witnessed by a third party such as TUV, BV, SGS, DNV or Lloyd's Register is available on request. Ultrasonic testing is carried out to EN 10228-3, SEP 1921 or ASTM A388 as specified.
How is 1.4568 machined?
Rough machine in Condition A, where machinability is close to austenitic grades 302 and 304, then finish machine after hardening with 0.3 to 0.8 mm per side left on. In the fully aged RH 950 and CH 900 conditions the material reaches 48 to 49 HRC and is difficult to turn, drill and tap. Carbide or ceramic tooling, rigid setups, reduced surface speed and generous coolant are required.
What is the maximum service temperature of 1.4568?
1.4568 holds useful mechanical properties in continuous service up to about 480 °C (900 °F). Above that the precipitation-hardened structure over-ages and strength falls, so a heat-resistant grade such as Inconel 617, Incoloy 800H or Incoloy 800HT is specified instead.
Can 1.4568 be used in seawater or sour service?
No. 1.4568 contains no molybdenum and its chloride pitting resistance is close to type 301, which is not enough for seawater, brine or H2S-bearing sour service. For those duties specify a duplex, super-duplex or nickel-alloy forging such as Incoloy 825 or Inconel 725. Fully aged high-strength conditions are also more susceptible to stress-corrosion cracking than Condition A.
What is the minimum order quantity and lead time for 1.4568 forgings?
Single-piece and prototype orders are accepted, because open-die forgings are made to the customer drawing rather than from a fixed die, so there is no tooling cost to amortise. Lead time is 25 to 45 days depending on section size, heat-treatment condition and testing scope. Send a drawing or the finished dimensions to sales@steelforgepieces.com for a quotation.
About the manufacturer
Jiangyin Jiangnan Metal Co., Ltd. is an open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, inside the Yangtze River Delta forging cluster and within two hours of the ports of Shanghai and Ningbo.
The factory produces open-die forgings and seamless rolled rings in carbon steel, alloy steel, tool steel, stainless steel and nickel alloys, covering forged rings, flanges, shafts, discs, sleeves, bushings, tube sheets, hollow bars and round bars from a few kilograms to multi-tonne single pieces. Work is supplied to EN, ASTM, ASME, DIN, JIS and GB specifications with EN 10204 3.1 or 3.2 certification, and exported to pressure-vessel, valve, pump, offshore, power-generation and heavy-machinery manufacturers worldwide.
Request a quotation for 1.4568 forgings
Send the drawing or the finished dimensions, the required heat-treatment condition (A, TH 1050 or RH 950), the quantity and the testing and certification scope. A quotation with weight, lead time and price normally follows within one working day.
Email sales@steelforgepieces.com Call 0086-189-2135-9659 Contact page
Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Related stainless steel and nickel alloy forgings
- 17-7 PH forgings, the trade-name page for this same alloy
- 17-4 PH (1.4542 / S17400) forgings, martensitic PH alternative for heavy sections
- PH 13-8 Mo (1.4534 / S13800) forgings, higher toughness and transverse properties
- Incoloy 825 forgings, for chloride and acid service beyond the limits of 1.4568
- Inconel X-750 forgings, precipitation-hardening nickel alloy for higher temperatures
- Inconel 617 forgings, for service well above the 480 °C limit of 1.4568
- All stainless steel forging grades