1. The grade
The designation follows the older French naming system. Z marks a high-alloy steel, 6 stands for about 0.06 percent carbon, C N D T are chromium, nickel, molybdenum and titanium, and 17-12 gives the nominal chromium and nickel contents.
Two alloying additions define the grade. Molybdenum at 2.0 to 2.5 percent lifts resistance to pitting and crevice attack above that of a plain 18/10 steel. Titanium is a stronger carbide former than chromium and holds carbon as TiC, so chromium stays in solution through welding and through the 425 to 815 C sensitisation range. That is why the grade can be welded without a solution anneal afterwards for corrosion reasons.
2. Equivalent grades and governing standards
| System or country | Designation |
|---|---|
| France, AFNOR NF | Z6CNDT17-12, Z6CNT17-12, Z8CNDT17-12 |
| EN, Werkstoff | X6CrNiMoTi17-12-2, 1.4571 |
| Germany, DIN | X6CrNiMoTi17-12-2, X10CrNiMoTi18-10 |
| USA, AISI and UNS | 316Ti, TP316Ti, UNS S31635 |
| Japan, JIS | SUS316Ti, 316Ti |
| UK, BS | 320S31, 320S18, 321S12 |
| Italy, UNI | X6CrNiMoTi17-12 |
| China, GB | 0Cr18Ni12Mo2Ti, 1Cr18Ni12Mo2Ti, 06Cr17Ni12Mo2Ti |
| Sweden, SS | 2350, 2350-02 |
| Poland, PN | H17N13M2T |
| Czechia, CSN | 17348 |
| Russia, GOST | 08Kh17N13M2T, 10Kh17N13M2T |
| Spain, UNE | F.3535 |
| Standard | Scope |
|---|---|
| NF A36-607 | Austenitic stainless steel parts obtained by flat die forging or drop forging for boilers and pressure vessels, grades and types. Cancelled. |
| NF A35-574 | Stainless steel for general purposes, semi-finished products, bars and wire rod |
| NF A35-573 | Stainless steels for general purposes, plates, wide strips and strips |
| NF A35-578 | Stainless steel for high-temperature application |
| NF A36-209 | Austenitic and austenitic-ferritic stainless steel plates for boilers and pressure vessels |
| EN 10088-3 | Stainless steels, semi-finished products, bars, rods, wire, sections and bright products, grade 1.4571 |
| EN 10222-5 | Steel forgings for pressure purposes, martensitic, austenitic and austenitic-ferritic stainless steels |
| ASTM A182, ASME SA-182 | Forged or rolled alloy and stainless steel pipe flanges, forged fittings, valves and parts, Grade F316Ti |
3. Chemical composition
The three systems are equivalent, not identical. The AFNOR window is the tightest on carbon, silicon and nickel. ASTM is the widest on molybdenum and nickel. A heat that passes 1.4571 can fail Z6CNDT17-12 on carbon or nickel, so the governing standard has to be fixed before the melt is booked.
| Element | AFNOR Z6CNDT17-12 | EN 1.4571, X6CrNiMoTi17-12-2 | ASTM 316Ti, UNS S31635 |
|---|---|---|---|
| C | 0.060 max | 0.08 max | 0.08 max |
| Si | 0.75 max | 1.00 max | 1.00 max |
| Mn | 2.00 max | 2.00 max | 2.00 max |
| P | 0.040 max | 0.045 max | 0.045 max |
| S | 0.015 max | 0.015 max, see note | 0.030 max |
| N | 0.020 max | not specified | not specified |
| Cr | 16.00 to 18.00 | 16.5 to 18.5 | 16.0 to 18.0 |
| Ni | 10.50 to 12.50 | 10.5 to 13.5 | 10.0 to 14.0 |
| Mo | 2.00 to 2.50 | 2.00 to 2.50 | 2.0 to 3.0 |
| Ti | 5 x (C+N) min, 0.70 max | 5 x C min, 0.70 max | 0.70 max |
| Fe | Balance | ||
Published EN data sheets differ on the sulphur ceiling for 1.4571. Both 0.015 and 0.030 percent appear in circulation. Confirm against the edition of EN 10088-3 being purchased to.
4. Mechanical properties at room temperature
Values are for the solution-annealed condition. Forgings are tested on a representative test piece under the governing standard.
| Property | EN 10088-3, 1.4571, dia 160 mm or less | Published 316Ti and Z6CNDT17-12 data |
|---|---|---|
| Tensile strength Rm | 500 to 700 MPa | 515 MPa min |
| Proof strength Rp0.2 | 200 MPa min | 205 MPa min |
| Proof strength Rp1.0 | 235 MPa min | not stated |
| Elongation A, longitudinal | 40 percent min | 40 percent min in 50 mm |
| Hardness | 215 HB max | not stated |
| Impact energy KV at 20 C | 100 J min, drawn bar | not stated |
| Form | Rm, MPa | Rp0.2, MPa | A, percent |
|---|---|---|---|
| Hot-rolled peeled bar | 500 to 700 | over 200 | not stated |
| Drawn bar | 500 to 950 | over 200 | over 25 |
| Hot-rolled plate | 520 to 670 | over 220 | over 40 |
| Cold-rolled strip | 540 to 690 | over 240 | over 40 |
| Seamless hot-rolled tube | not stated | over 190 | over 40 |
5. Proof strength at elevated temperature
Solution-annealed condition. These are the figures a pressure vessel or piping designer needs when the part runs hot.
| Temperature, C | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 |
|---|---|---|---|---|---|---|---|---|---|---|
| Rp0.2 min | 185 | 175 | 165 | 155 | 145 | 140 | 135 | 131 | 129 | 127 |
| Rp1.0 min | 215 | 205 | 192 | 183 | 175 | 169 | 164 | 160 | 158 | 157 |
Published data gives a maximum service temperature of about 550 C for this grade, and notes that 316Ti can be held in service for long periods at up to 500 C without loss of corrosion resistance. The grade is also suitable for low-temperature service.
6. Physical properties
| Property | Value | Unit |
|---|---|---|
| Density | 8.0 | kg/dm3 |
| Modulus of elasticity | 200 | GPa |
| Thermal conductivity | 15 | W/m.K |
| Specific heat capacity | 500 | J/kg.K |
| Electrical resistivity | 0.75 | ohm.mm2/m |
| Magnetisability | low, relative permeability 1.3 max | - |
| PREN | 23.1 to 26.7 | - |
Thermal conductivity is low and thermal expansion is high, so thin sections distort more readily than carbon steel during heating and quenching. This shows up on long shafts and thin-walled rings during heat treatment. Although the structure is austenitic, the grade can show some magnetic response, so a magnet is not a reliable way to identify it.
7. Corrosion behaviour
Intergranular corrosion
Resistant both as delivered and as welded. Titanium ties up carbon, so chromium carbides do not precipitate at grain boundaries.
Pitting and crevice
Better than 1.4301 because of the molybdenum addition. PREN 23.1 to 26.7.
Seawater and high chloride
Not resistant, pitting can occur. For seawater duty use a 6 Mo grade such as A182 F44 or a duplex such as F51.
Acids
Resistant to organic acids such as formic acid, and to sulphuric acid in low and medium concentrations, within the limits of the published data.
8. Forging and heat treatment
| Operation | Temperature | Cooling |
|---|---|---|
| Heating for forging | 1150 to 1180 C | - |
| Forging range | 1180 down to 950 C, hot forming cited as 1200 down to 900 C | Water after forging, air after hot forming |
| Solution annealing | 1020 to 1120 C | Water or air, rapid |
Forgeability is good and the grade suits both open-die forging and drop forging. In our shop the forging is cogged or ring-rolled from an on-site melt, returned to the furnace as often as the reduction schedule needs, then solution annealed in one of fourteen heat treatment furnaces. Soak time is set by ruling section. Long shafts are quenched vertically in a 15 m well-type furnace to hold distortion down, which matters for a steel with this expansion coefficient.
9. Welding and machining
Welding
Good weldability with all common processes except gas welding. A filler metal is not strictly required. Where one is used, 1.4430 is a commonly recommended choice. Post-weld heat treatment is not needed and welding does not impair resistance to intergranular corrosion. In bare-wire processes much of the titanium is lost across the arc, which is why matching or niobium-stabilised fillers are often specified.
Machining
Moderate to poor, and worse than other chromium-nickel-molybdenum stainless steels. Titanium carbonitrides form during cutting and accelerate tool wear. This is not a free-machining grade and it is the wrong choice for demanding high-speed machining. Rigid setups, sharp positive-rake tooling and a steady feed that keeps the tool below the work-hardened layer are the usual measures. Cold forming and cold pressing present no particular difficulty.
10. Forged product forms in Z6CNDT17-12
| Form | Typical parts | Size envelope |
|---|---|---|
| Seamless rolled rings | Ring blanks, bearing rings, retaining rings, flange blanks, contoured rings | OD 50 to 6,000 mm |
| Forged rings | Valve seat rings, gear rings, heavy sections outside the mill envelope | Upset and punch route |
| Forged flanges | Weld neck, blind, slip-on, socket weld, lap joint, orifice, long weld neck | ASME B16.5, B16.47, API 6A |
| Shafts and spindles | Stepped shafts, eccentric shafts, valve stems, pins, rolls | to 14,000 mm turned length |
| Bars, blocks and blanks | Round, flat and square bar, gear blanks, wheels, manifolds | per drawing |
| Discs and tube sheets | Solid discs, tube sheets, covers, blind plates, hubs | to 5,000 mm machined |
| Cylinders, sleeves, bushings | Hollow cylinders, liners, couplings, heavy-wall pipe sections | bore to 1,600 x 10,000 mm |
| Valve and pump parts | Bodies, bonnets, blocks, seat rings, nozzles, spools | per drawing |
Supplied as forged with machining allowance, proof-machined for ultrasonic inspection, or finish-machined to drawing. Single pieces up to 30 tonnes. Minimum order 10 kg with no minimum piece count, so a one-off replacement part can be quoted.
11. Where the grade is used
Chemical and petrochemical
Pressure vessel flanges, tube sheets, covers, nozzles, chemical transport containers, heat exchanger components, piping parts in contact with process chemicals.
Oil, gas and offshore
Subsea and deepwater production hardware, compressor and generator components, spools and valve parts.
Pulp, paper and refining
Digesters, liquor tanks, paper machine components, refinery catalytic recovery systems and recuperators.
Food and pharmaceutical
Food preparation and storage equipment, in particular in acidic environments, and pharmaceutical production hardware.
Marine and shipbuilding
Apparatus engineering, pipeline construction and shipbuilding components, covered by CCS, BV, DNV, LR and NK approvals.
Power and rotating equipment
Turbine and gas compressor parts, gearbox blanks, power transmission rings, pressure vessel and pipeline construction.
12. Testing, inspection and certification
Because the steel is melted here, chemistry is verified at the furnace rather than inherited from a billet supplier certificate, and the melt number follows the part through forging, heat treatment, machining and shipment.
| Test | Method or standard | Scope |
|---|---|---|
| Chemical analysis | ASTM E415 optical emission, ASTM E1019 for C and S | Every heat, in house |
| Tensile | ASTM A370, ISO 6892 | Every order, in house |
| Impact, Charpy V | ASTM A370, down to minus 60 C | On request, in house |
| Ultrasonic testing | ASTM A388, EN 10228-3, SEP 1921 | To the class stated on the order |
| Magnetic particle, PMI | ASTM E709, handheld alloy analyser | On request |
| Grain size and metallography | ASTM E112 | On request |
| Intergranular corrosion | ASTM A262, ASTM G28 | Accredited third-party laboratory |
| Pitting resistance | ASTM G48 | Accredited third-party laboratory |
| Certificate | EN 10204 3.1 standard, 3.2 witnessed by BV, DNV, LR, SGS, TUV or your inspector | Every shipment |
13. The plant behind the part
Most forging suppliers in China buy billet. This works melts its own steel, which for a titanium-stabilised grade is a metallurgical point rather than a sales one, since the titanium aim and the carbon plus nitrogen balance are set in our ladle instead of being accepted as delivered.
| Stage | Equipment | Capacity |
|---|---|---|
| Melting | Electric arc furnace, ladle furnace, vacuum oxygen decarburisation | 60 t max heat, VOD 30 t and 60 t |
| Remelting, optional | Protective-atmosphere ESR, VIM, VAR | ESR 3 t and 6 t, VIM 3 t, VAR 6 t |
| Forging | Hydraulic open-die presses, hammers | 6,300 t, 4,000 t, 2,000 t, hammers 750 kg to 5 t |
| Ring rolling | Radial-axial ring mills | 6 m, 3 m, 1 m, max OD 6,000 mm |
| Heat treatment | 14 furnaces, including 3 high-temperature and 2 well-type | chamber to 8,000 x 2,000 x 2,000 mm, 15 m deep pit |
| Machining | Vertical and horizontal lathes, CNC, deep-hole drilling | 5,000 mm swing, 14 m centres, bore 1,600 x 10,000 mm |
Operating since 1997 with 460 staff, including 9 senior engineers and 32 intermediate engineers. Class approvals CCS, BV, DNV, LR and NK. Exports to North America, Europe, the Middle East and Asia-Pacific.
14. Request a quotation
A price comes back within two working days of a complete enquiry. Six items are what the estimator needs. Anything missing means a round trip of questions first.
| No. | Item | Example |
|---|---|---|
| 1 | Grade and governing standard | Z6CNDT17-12 to AFNOR limits, or 1.4571 to EN 10222-5 |
| 2 | Dimensions or drawing | OD 1200 x ID 900 x H 260 mm, PDF, DWG, DXF, STEP |
| 3 | Quantity and repeat volume | 12 pieces, about 4 times per year |
| 4 | Delivery condition | As forged, proof-machined or finish-machined |
| 5 | Heat treatment and testing | Solution annealed 1050 C water quench, UT to ASTM A388, ASTM A262 Practice E |
| 6 | Certification and destination | EN 10204 3.2 witnessed by DNV, Rotterdam |
Jiangyin Jiangnan Metal Co., Ltd.
Open-die forging factory with its own melt shop, established 1997.
Plant
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, 214423
Phone
+86 189 2135 9659
Monday to Saturday, 08:00 to 17:30, UTC+8
sales@steelforgepieces.com
English and Chinese
Terms
Minimum order 10 kg, lead time 20 to 60 days, quotation in 2 working days, EN 10204 3.1 or 3.2
15. Questions we are asked about this grade
What is Z6CNDT17-12 steel?
It is the AFNOR designation for a titanium-stabilised austenitic chromium-nickel-molybdenum stainless steel. The European equivalent is X6CrNiMoTi17-12-2, material number 1.4571. The American equivalent is AISI 316Ti, UNS S31635. Titanium at five times the carbon content binds carbon as titanium carbide, so the steel resists intergranular corrosion in the as-welded condition, and molybdenum at 2.0 to 2.5 percent improves pitting and crevice resistance over 1.4301.
Is Z6CNDT17-12 the same as 1.4571 and 316Ti?
Equivalent, not identical. AFNOR limits carbon to 0.060 percent, silicon to 0.75 percent, chromium to 16.0 to 18.0 and nickel to 10.5 to 12.5. EN 1.4571 allows carbon to 0.08 percent, silicon to 1.00 percent, chromium 16.5 to 18.5 and nickel 10.5 to 13.5. ASTM 316Ti allows molybdenum to 3.0 percent and nickel to 14.0 percent. A heat certified to 1.4571 does not automatically meet the narrower AFNOR window, so name the governing standard on the purchase order.
What is the chemical composition of Z6CNDT17-12?
To the AFNOR limits: C 0.060 max, Si 0.75 max, Mn 2.00 max, P 0.040 max, S 0.015 max, Cr 16.00 to 18.00, Mo 2.00 to 2.50, Ni 10.50 to 12.50, N 0.020 max, Ti from 5 x (C+N) up to 0.70 percent, balance iron.
What are the mechanical properties of forgings in this grade?
Solution annealed, per EN 10088-3 for the 1.4571 equivalent: tensile 500 to 700 MPa, Rp0.2 200 MPa min, Rp1.0 235 MPa min, elongation 40 percent min longitudinal, hardness 215 HB max. Data published for the ASTM 316Ti equivalent is quoted as 515 MPa tensile min, 205 MPa yield min and 40 percent elongation.
How is Z6CNDT17-12 forged and heat treated?
Heat to 1150 to 1180 C and forge between 1180 and 950 C, then cool. Solution anneal at 1020 to 1120 C with rapid cooling in water or air. Open-die forging and drop forging are both suitable.
What is the maximum service temperature?
Published data gives about 550 C as the maximum service temperature, with long-term exposure up to 500 C without loss of corrosion resistance. The grade is also suitable for low-temperature service.
Can it be welded without post-weld heat treatment?
Yes. The 1.4571 equivalent welds with all common processes except gas welding, needs no post-weld heat treatment, and does not lose resistance to intergranular corrosion through welding. Where a filler is used, 1.4430 is a commonly recommended choice.
Why is this grade hard to machine?
Titanium carbonitrides form during cutting and are abrasive, so tool wear is higher than with other chromium-nickel-molybdenum stainless steels. Machinability is rated moderate to poor. It is not a free-machining grade and is a poor choice for demanding high-speed machining.
Will it work in seawater?
No. The grade is not resistant to seawater and salt and pitting can occur. For seawater and high-chloride duty, consider a 6 Mo austenitic such as A182 F44 or 904L, or a duplex grade such as F51 or F53.
Who supplies Z6CNDT17-12 open-die forgings in China?
Jiangyin Jiangnan Metal Co., Ltd., an integrated melting and open-die forging works at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. The plant melts its own steel by EAF, ladle furnace and VOD, with ESR, VIM and VAR remelting available, rolls rings to 6,000 mm outside diameter, forges single pieces to 30 tonnes, holds CCS, BV, DNV, LR and NK approvals, and issues EN 10204 3.1 or 3.2 certificates with ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388. Minimum order 10 kg. Contact +86 189 2135 9659 or sales@steelforgepieces.com.
What is the minimum order and lead time?
Minimum order is 10 kg with no minimum piece count, so a single part can be quoted. Lead time is normally 20 to 60 days from order confirmation, with a standard stainless grade such as this one at the lower end and remelted grades at the upper end. Quotations are returned within two working days of a complete enquiry.
Sources and revision
Composition and property data on this page is compiled from the AFNOR designation tables for NF A36-607 and NF A35-574, from EN 10088-3 data published for X6CrNiMoTi17-12-2 (1.4571), and from ASTM data published for 316Ti, UNS S31635. Values differ between the three systems and are labelled accordingly. Figures are given for guidance and do not replace the purchased standard or a project specification.
Issued by the engineering department of Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Telephone +86 189 2135 9659. Email sales@steelforgepieces.com.
Document JN-SS-Z6CNDT1712. Last reviewed 11 October 2026.