Page last reviewed . Published by Jiangyin Jiangnan Metal Co., Ltd.
XM-28 at a glance
- Grade: XM-28 (UNS S24100) is a nitrogen-strengthened, low-nickel austenitic stainless steel in which manganese and nitrogen take the place of most of the nickel used in Type 304.
- Strength: annealed minimums to ASTM A276 are 690 MPa (100 ksi) tensile and 379 MPa (55 ksi) 0.2% yield, about double the yield of annealed 304.
- Corrosion: close to Type 304 in weak acids and pitting media, below 304 in more aggressive media.
- Magnetic permeability: about 1.008 annealed and 1.011 after 70% cold drawing (H = 200 Oe, 70 F).
- Hardening: by cold work only. The grade does not respond to hardening heat treatment.
- Forged forms we make: rings, rolled rings, flanges, shafts, discs, bushings, sleeves, tube sheets, blocks and bars, 10 kg to 20 t, to customer drawing.
1. Chemical composition of XM-28 / UNS S24100
XM-28 belongs to the Cr-Mn-N group of austenitic stainless steels. The high manganese content holds the austenite stable so nickel can be kept to 0.5-2.5%, and 0.20-0.45% nitrogen provides the interstitial solid-solution strengthening the grade is bought for.
| Element | Symbol | Content (%) | Function |
|---|---|---|---|
| Carbon | C | 0.15 max | Strength; limits intergranular corrosion resistance |
| Chromium | Cr | 16.5 - 19.5 | Passive film, corrosion resistance |
| Manganese | Mn | 11.0 - 14.0 | Austenite stabiliser, raises nitrogen solubility |
| Nickel | Ni | 0.50 - 2.50 | Austenite stabiliser, deliberately low |
| Nitrogen | N | 0.20 - 0.45 | Main strengthening element |
| Silicon | Si | 1.00 max | Deoxidiser |
| Phosphorus | P | 0.045 - 0.06 max | Residual, limit depends on specification |
| Sulphur | S | 0.030 max | Residual |
| Iron | Fe | Balance | Matrix |
Ranges follow published mill data for UNS S24100. Producer sheets state chromium as either 16.50-19.00 or 16.50-19.50, and phosphorus as either 0.045 max or 0.06 max. The governing limits are those of the purchase specification (ASTM A276, A314, A313 or A580), and we certify to the limits stated on your order.
2. Mechanical properties, annealed
| Property | Metric | Imperial | Basis |
|---|---|---|---|
| Ultimate tensile strength | 690 MPa | 100 ksi | ASTM A276 min |
| Yield strength, 0.2% offset | 379 MPa | 55 ksi | ASTM A276 min |
| Elongation | 30 % | 30 % | ASTM A276 min |
| Reduction of area | 50 % | 50 % | ASTM A276 min |
| Hardness | about 92 HRB | about 92 HRB | Typical, annealed |
Annealed Type 304 is normally specified at 515 MPa tensile and 205 MPa yield, which is the basis for the standard statement that XM-28 carries about twice the yield strength of 304. Cold-worked product runs much higher. Drawn and cold-headed XM-28 wire is commonly supplied in the 827-965 MPa (120-140 ksi) tensile range.
3. Physical properties
| Property | Value | Condition |
|---|---|---|
| Density | 7.78 - 7.83 g/cm3 (0.281-0.283 lb/in3) | Producer sheets differ slightly |
| Melting range | 1418 - 1510 C (2585 - 2750 F) | Range spans published data |
| Modulus of elasticity | 200 GPa (29 x 10⁶ psi) | at 21 C / 70 F |
| Specific heat | 0.12 Btu/lb·F | 0-100 C / 32-212 F |
| Electrical resistivity | 27.6 microhm-in | at 21 C / 70 F |
| Magnetic permeability | 1.008 annealed, 1.011 at 70% cold drawn | H = 200 Oe, 70 F |
| Thermal expansion | 9.4 x 10⁻⁶ /F (23-204 C) | 10.7 x 10⁻⁶ to 649 C; 11.6 x 10⁻⁶ to 982 C |
4. Forging, heat treatment and fabrication
Forging and hot working
Charge and soak to about 1177 C (2150 F), finish forging at about 1093 C (2000 F). Published practice gives a hot working window of roughly 1121-1204 C (2050-2200 F), with in-process annealing at 1038-1093 C (1900-2000 F). The grade work hardens quickly, so reheats are planned into the pass schedule. We set the schedule around the final ring or shaft geometry so that grain flow follows the part contour.
Annealing
XM-28 does not harden by heat treatment. Solution anneal at 1038-1121 C (1900-2050 F), with 1066 C (1950 F) the common mill practice, then cool rapidly in water or air. Strength above the annealed level is obtained only by cold work.
Welding
Weldable by GTAW, GMAW, SMAW and submerged-arc processes. Preheat is not required.
Machining
Machining behaviour is similar to Type 304, but the higher strength and strong work hardening call for lower cutting speeds, positive feeds, rigid set-ups and sulphurised cutting oil. Machinability is rated at roughly 30% of AISI B1112.
5. Specifications and designations
| Standard | Product form covered |
|---|---|
| ASTM A314 | Stainless steel billets and bars for forging |
| ASTM A276 / A276M | Stainless steel bars and shapes, hot or cold finished (Type XM-28) |
| ASTM A313 | Stainless steel spring wire |
| ASTM A580 | Stainless steel wire |
| UNS | S24100 |
| Trade name | Nitronic 32, a registered trademark of AK Steel |
Where bars and shapes are used in boiler and pressure-vessel work, ASTM A479 is the usual companion to A276. Check that the grade is listed in the edition of A479 your project works to before specifying it.
7. Where XM-28 is used
The grade is chosen where high strength, low magnetic permeability and 304-class corrosion resistance are wanted without paying for nickel. Published application lists for UNS S24100 include the following.
Pole line and utility hardware
Clamps for pole line hardware and skid wire for underground transmission lines. Strength plus very low magnetic permeability.
Concrete reinforcing accessories
Reinforcing accessories and cold-headed parts that must hold high mechanical properties.
Shafting and dam gate stems
Forged shafts, spindles and dam gate stems for water control structures.
Screens, racks and cages
Abrasion and corrosion resistant screens, racks and cages in bulk handling and process plant.
Non-magnetic springs and wire forms
High strength non-magnetic springs and wire forms made from A313 and A580 product.
Fasteners and cold-headed parts
Fasteners and communication hardware, the long-standing cold-heading use for this grade.
The examples above follow published producer data for UNS S24100. Suitability for a given service has to be confirmed by the design authority. Send us your duty conditions and we will say when a different grade is the safer choice.
8. What we forge in XM-28
Jiangyin Jiangnan Metal Co., Ltd. is an open-die forging factory. Every XM-28 item is made to the customer drawing or dimension sheet, so there is no fixed size catalogue.
Rolled rings
Ring-rolled blanks and finish-machined rings, plain or profiled.
Forged flanges
Weld neck, slip on, blind and special profile flanges forged from solid.
Shafts and spindles
Straight, stepped and eccentric shafts, spindles and stems.
Discs and blocks
Upset discs, hubs, blanks and rectangular blocks.
Sleeves and bushings
Hollow forged and trepanned sleeves, bushings and cylinders.
Round bars and tube sheets
Forged round bar, tube sheets and heavy plate-type forgings.
Melting, testing and certification
We melt XM-28 by EAF + VOD, with ESR remelting available where cleanliness or segregation control matters. Non-destructive testing is agreed per order. For this austenitic grade the correct ultrasonic standard is EN 10228-4, ultrasonic testing of austenitic and austenitic-ferritic stainless steel forgings. EN 10228-3 covers ferritic and martensitic forgings and does not apply here. ASTM A388/A388M contact pulse-echo examination can be applied to heavy forgings. Material certificates are issued to EN 10204 type 3.1, or type 3.2 countersigned by an independent inspectorate when the purchase order calls for it.
9. Questions we are asked about XM-28
What is XM-28 stainless steel?
Is XM-28 the same as Nitronic 32?
What tensile and yield strength should be expected?
Can XM-28 be hardened by heat treatment?
Is XM-28 suitable for seawater, sour service or strong acids?
Is XM-28 magnetic?
Which ultrasonic standard applies to XM-28 forgings?
What do you need in order to quote?
10. Basis of the data
Chemistry, mechanical and physical data on this page are taken from published mill and producer data sheets for UNS S24100 together with the governing ASTM specifications A276, A314, A313 and A580. Where producer sheets disagree, on the chromium upper limit, the phosphorus limit, melting range and density, both figures are shown rather than averaged. Values are typical and are not a warranty of properties for any particular application. The binding values for an order are those on the mill certificate issued against the purchase specification.