X2CrMoTi18-2 Forgings, EN 1.4521 / AISI 444 / UNS S44400
Forged round, square, flat and hexagonal bar, hollow bar, sleeve, bush, cylinder and shell, forged and seamless rolled rings, discs, blocks and plates, all made to drawing at our works in Jiangyin, China.
Datasheet reviewed 9 October 2026. Values are taken from published grade datasheets listed under references.
Grade at a glance
X2CrMoTi18-2 (EN material number 1.4521) is a low carbon ferritic chromium stainless steel with molybdenum added. Chromium runs 17 to 20 %, molybdenum 1.80 to 2.50 %, carbon is held at 0.025 % maximum and the structure is stabilized with titanium. It contains no nickel and is the European equivalent of AISI 444, UNS S44400 and JIS SUS444. Corrosion resistance is quoted as equal to 1.4401 and 1.4404 (316 and 316L), with excellent resistance to chloride stress corrosion cracking. Annealed proof strength is 320 N/mm² minimum with tensile 450 to 650 N/mm², the steel is magnetizable, and it is forged from 1050 down to 750 °C and annealed at 750 to 900 °C.
- EN 1.4521
- EN name X2CrMoTi18-2
- AISI 444
- UNS S44400
- JIS SUS444
- Structure ferritic
- Nickel none
- Magnetic yes
1. Designations and equivalent grades
| System | Designation | Remark |
|---|---|---|
| EN, Europe | 1.4521, X2CrMoTi18-2 | Listed in EN 10088-2 and EN 10028-7 |
| AISI / SAE, USA | 444 | |
| UNS, USA | S44400, also listed as S44401 | S44401 covers the Ti and Nb stabilized variant |
| JIS, Japan | SUS444 | |
| China | 019Cr19Mo2NbTi, 00Cr18Mo2 | Current and former designations |
| SS, Sweden | 2326 | |
| UNE, Spain | F-3123 | |
| NF, France | Z3CDT18-02, Z3CDFT18-02 | |
| STAS, Romania | 2TiMoCr180 | |
| Mill name | Supra 444/4521 | Outokumpu trade name for the grade |
| Related, not interchangeable | 1.4523 (X2CrMoTiS18), 1.4605 (X2CrAlTi18-2) | 1.4523 carries 0.15 to 0.35 % sulphur for machinability, 1.4605 is aluminium stabilized without molybdenum |
2. Chemical composition
| Specification | C | Si | Mn | P | S | Cr | Mo | N | Ti |
|---|---|---|---|---|---|---|---|---|---|
| EN 1.4521 | max 0.025 | max 1.00 | max 1.00 | max 0.040 | max 0.015 | 17.0 to 20.0 | 1.80 to 2.50 | max 0.030 | 0.15 to 0.80, to 4 x (C + N) + 0.15 |
| AISI 444, S44400 / S44401 | max 0.030 | max 1.00 | max 0.50 | max 0.040 | max 0.030 | 17.5 to 19.5 | 1.75 to 2.50 | max 0.035 | Ti and Nb stabilized |
| JIS SUS444 | max 0.025 | max 1.00 | max 1.00 | max 0.040 | max 0.030 | 17.0 to 20.0 | 1.75 to 2.50 | max 0.025 | stabilized |
| Typical mill analysis | 0.02 | 18 | 2 | Nb and Ti |
Balance iron. Using both titanium and niobium gives a fully stabilized ferritic structure at a lower titanium level, which helps surface quality on the finished part.
3. Mechanical properties, annealed
| Basis and product form | Rp0.2 (N/mm²) | Rm (N/mm²) | Elongation |
|---|---|---|---|
| EN 10088-2, cold rolled coil and sheet | min 320 | 420 to 640 | A80 min 20 % |
| EN 10088-2, hot rolled coil and sheet | min 300 | 400 to 600 | A80 min 20 % |
| EN 10088-2, quarto plate | min 300 | 420 to 620 | A min 20 % |
| Supplier datasheet value, Metalcor | min 320 | 450 to 650 | A5 min 20 % |
| Hardness | max 200 HB30 (Metalcor), max 185 HB (Virgamet) | ||
| Modulus of elasticity at 20 °C | 220 kN/mm² | ||
Ferritic grades of this type carry higher proof strength than the common austenitics while keeping elongation around 20 %. Properties actually achieved in a forging depend on section size, forging reduction, test position and the annealing cycle, so the acceptance values are fixed on the order rather than taken from flat product tables.
4. Physical properties at 20 °C
| Property | Value |
|---|---|
| Density | 7.7 g/cm³ |
| Modulus of elasticity | 220 kN/mm² |
| Specific heat capacity | 430 J/(kg K) |
| Thermal conductivity | 23 W/(m K) |
| Electrical resistivity | 0.8 Ω mm²/m |
| Magnetizable | Yes, ferritic structure |
5. Corrosion behaviour
The combination of 18 % chromium with 2 % molybdenum is what lifts this grade above the plain 17 % chromium ferritics. Metalcor records corrosion resistance equal to 1.4401 and 1.4404, the 316 and 316L austenitics, together with excellent resistance to stress corrosion cracking caused by chlorides. Outokumpu describes resistance to localized corrosion as close to the 1.4401 acid proof austenitic for its 18 % chromium, 2 % molybdenum ferritic product. Taking the pitting resistance equivalent in its usual form, Cr + 3.3 Mo, the typical analysis of 18 % chromium and 2 % molybdenum gives roughly 25.
In chloride bearing solutions pitting and crevice attack are still possible, and the outcome depends on chloride concentration, temperature, pH, redox potential and crevice geometry. Service life is usually decided by details rather than by the grade alone: avoid stagnant crevices in the design, pickle or mechanically clean weld and forging scale, and clean the surface at intervals where the duty allows it.
The practical argument for choosing 1.4521 over 304 or 316 is the resistance to chloride stress corrosion cracking, which is the failure mode that restricts austenitic grades in warm chloride service, together with the absence of nickel.
6. Forging and heat treatment
| Operation | Temperature | Cooling |
|---|---|---|
| Open-die forging | 1050 down to 750 °C | Water, air or gas |
| Hot rolling | 1050 down to 750 °C | Water, air or gas |
| Annealing | 750 to 900 °C | Air or gas, furnace cooling only in special cases |
| Hardening | Not possible, ferritic grade, strength comes from composition and the annealed condition | |
Our route for this grade
Certified billet or ingot with stabilized chemistry is soaked, then upset and drawn inside the 1050 to 750 °C window on our hydraulic presses, or ring rolled where the item is a ring. Work is reheated rather than finished below the bottom of the range, and time at the top of the range is kept short because ferritic steels coarsen if held hot. The piece is then annealed between 750 and 900 °C with air or gas cooling, rough machined, and checked for dimensions, chemistry by spectro or PMI, hardness and tensile properties. Certification is EN 10204 3.1 as standard. Ultrasonic testing, dye penetrant, extra tensile positions, impact testing and third party inspection by SGS, BV or TUV are added when the order calls for them.
7. Welding, machining and forming
Welding
Metalcor gives filler metal 1.4430, the 316L type, as suitable for this grade. Keep heat input low, use clean inert shielding, and remove weld oxide by pickling or mechanical cleaning so that the passive film reforms. Expect lower ductility across the weld than in the parent metal, and treat heavy sections with more care than thin ones.
Machining
The grade work hardens far less than the austenitics, so chip control and tool life are more predictable. Use sharp tooling, a rigid set-up and plenty of coolant. Where free cutting behaviour matters more than corrosion performance, 1.4523 is the sulphur bearing relative, but it should not be substituted without agreement because sulphur lowers corrosion resistance.
Cold forming
Stabilized 18 % chromium ferritics bend, fold and draw well, and Outokumpu describes its 444/4521 product as having excellent deep drawability. On forged items this matters mainly for downstream operations such as flaring or swaging on hollow bar.
8. Where the grade is used
Metalcor lists cold heading parts and heat exchanger tubes as the applications for 1.4521, and the grade is supplied by mills mainly as sheet, plate, tube and fittings. Wider literature for the 18 % chromium, 2 % molybdenum ferritic covers hot water tanks and water heaters, heat exchangers, boiler and flue components, solar water heating, and pipework for water service. In forged form we most often make valve and pump parts, flange and ring blanks, tube sheet hardware, sleeves and shafts for hot water and brackish water duty, and nickel free parts for customers who have specified the grade to avoid chloride stress corrosion cracking.
One point worth raising early in an enquiry: potable water approvals such as the German DVGW or Swiss SVGW marks are granted to a named manufacturer for a named product and production route, never to a steel grade in general. If your project needs a specific approval, tell us at enquiry stage and we will confirm in writing what certification can be supplied with the forged item.
9. Forged product forms
| Form | Covers | Usual condition |
|---|---|---|
| Bar | Round bar and rod, square, rectangular, flat and hexagonal bar | Annealed, black or rough turned, cut to length |
| Hollow sections | Hollow bar, sleeve, bush, cylinder, barrel, casing, shell, hub, housing, pipe and tube blanks | Annealed, bored and rough machined |
| Rings | Forged rings, seamless rolled rings, flange blanks, wear and retaining rings | Annealed, faces rough machined |
| Discs and blocks | Discs, blanks, blocks, plates, slabs, stepped shafts | Annealed, saw cut or rough machined |
| To drawing | Shafts, stems, bodies, bonnets, tube sheets, near net shapes | As specified on the drawing |
10. Standards and basis of supply
The grade appears in EN 10088-2 for sheet, plate and strip and in EN 10028-7 for stainless flat products for pressure purposes, and as Type 444 UNS S44400 in ASTM A240. Because the published product forms are flat products, tube and fittings, forged bars, rings and shaped parts in this grade are normally ordered against agreed technical delivery conditions: chemistry to EN 10088, plus the mechanical values, test positions, heat treatment condition and testing set by the purchaser, often framed by EN 10250-4 for stainless open-die forgings or by ASTM A182. We state the exact basis on the quotation and repeat it on the certificate so that nothing is open to argument at incoming inspection.
11. Questions we are asked
What is X2CrMoTi18-2?
Is it as corrosion resistant as 316?
What temperatures are used for forging and annealing?
Is it magnetic, and is there nickel in it?
Which filler metal for welding?
Will you make a single piece?
What certification comes with the material?
12. Request a quotation
Send the drawing or specification for your X2CrMoTi18-2 bars, rings, hollow bars, discs or blocks and we will come back with price, forged weight and lead time.
Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, ChinaTel, WhatsApp and WeChat +86-189-2135-9659
Email sales@steelforgepieces.com
References
- Metalcor GmbH, datasheet 1.4521 / AISI 444 / UNS S44400: designations, composition, mechanical and physical properties, filler metal, applications. metalcor.de
- Virgamet, 1.4521, X2CrMoTi18-2, AISI 444, UNS S44401: equivalent grades, composition comparison, hardness, forging and annealing data. virgamet.com
- Outokumpu, Supra range datasheet, Supra 444/4521 (EN 1.4521, UNS S44400), November 2022: EN 10088-2 strength values, corrosion comparison, formability. outokumpu.com
- Steelnumber, X2CrMoTi18-2 / 1.4521 to EN 10088-2. steelnumber.com
- EN 10088-2, EN 10028-7, EN 10250-4 and ASTM A240 for the governing delivery conditions.
Figures above are standard minima or typical datasheet values for the grade and are given for guidance. They are not a guarantee of the properties of a particular forging, which depend on section size, reduction, test position and heat treatment as agreed on the order. Check requirements against the specification that governs your application.