GRADE X10CrNi18-8  /  EN 1.4310  /  UNS S30100 MELTED AND FORGED IN JIANGYIN, CHINA  /  EST. 1997 +86 189 2135 9659  /  sales@steelforgepieces.com
Jiangnan Metal Open-Die Forging Works Request Quote

HOME / STAINLESS STEEL / X10CrNi18-8

Austenitic Stainless Steel / Spring Grade

X10CrNi18-8EN 1.4310 · AISI 301 · UNS S30100 · open-die forgings, seamless rolled rings and flanges

X10CrNi18-8 is an austenitic chromium-nickel stainless steel carrying EN material number 1.4310, covered by EN 10088-1, EN 10088-2, EN 10088-3, EN 10151, EN 10263-5 and EN ISO 6931-1. It contains 0.05 to 0.15 % carbon, 16.0 to 19.0 % chromium and 6.0 to 9.5 % nickel. The nickel content is deliberately held low, which leaves the austenite metastable: the steel work hardens very quickly under cold deformation, and part of the structure turns to martensite as it does so. That single property explains almost everything else about the grade, from its use as a spring steel to its awkward machining behaviour.

We melt this grade ourselves rather than buying billet. Stainless heats run through the electric arc furnace, the ladle furnace and vacuum oxygen decarburisation, then go straight to the presses and the ring mill without leaving the site, so the certificate traces back to a melt number instead of stopping at a purchased bar.

Grade Summary1.4310
EN name
X10CrNi18-8
EN number
1.4310
US / UNS
AISI 301, UNS S30100
Structure
Austenitic, metastable
Density
7.9 kg/dm³
Rm annealed
500 to 700 MPa
Rp0.2 annealed
195 MPa minimum
Hardness
230 HB maximum
PREN
16.0 to 23.4
Forge range
1150–1200 °C down to 900 °C
Anneal
1000 to 1100 °C, rapid cool
Max service
300 °C as a spring
01

Chemical Composition

Composition limits follow EN 10088. Elements outside this list are not added deliberately, except as needed to finish the cast.

Table 1 — X10CrNi18-8 / 1.4310 chemical composition, mass %, to EN 10088
CSiMnPSCrNiMoN
0.05–0.15max 2.00max 2.00 max 0.045max 0.015 16.0–19.06.0–9.5max 0.80max 0.11

Molybdenum is not an alloying addition in this grade. The 0.80 % figure is a residual ceiling only, and a good deal of material published about 1.4310 gets this wrong. If the service condition needs molybdenum to resist chloride pitting, specify 904L, A182 F44 or a duplex grade such as A182 F51. We forge all of them.

The calculated pitting resistance equivalent runs from 16.0 to 23.4, depending on where chromium, molybdenum and nitrogen fall inside the band.

02

Equivalent Grades

Cross-references are listed below. The EN band is wider than AISI 301 on both chromium and nickel, so state the governing standard on the order where the distinction matters to the end user.

Table 2 — X10CrNi18-8 (1.4310) international equivalents
Region and standardDesignation
EU, EN 10088-3X10CrNi18-8 / 1.4310
USA, AISI and UNSAISI 301 (UNS S30100), AISI 302 (UNS S30200)
USA, AMSAMS 5516
Germany, DIN 17440, withdrawnX12CrNi17-7
Japan, JISSUS 301, SUS 302
United Kingdom, BS301S21, 302S26
France, AFNORZ11CN17-08, Z12CN18-09, Z12CN17-07
Sweden, SS2331
Russia, GOST12Kh18N9
Poland, PN1H18N9
Spain, UNEF-3507, X10CrNi18-9
Czech Republic17241, 17242
International, ISOX9CrNi18-8
03

Mechanical Properties

Values apply to the solution annealed condition at room temperature, tested longitudinally.

Table 3 — Mechanical properties, solution annealed
PropertySymbolValue
0.2 % proof strengthRp0.2195 MPa minimum
1.0 % proof strengthRp1.0230 MPa minimum
Tensile strengthRm500 to 700 MPa
Elongation at fractureA40 % minimum
Brinell hardnessHB230 maximum
Modulus of elasticity, 20 °CE200 GPa

Proof strength at temperature

Table 4 — Elevated temperature proof strength, solution annealed
Temperature100 °C150 °C200 °C250 °C300 °C
Rp0.2, MPa210200190185180
Rp1.0, MPa230215205200195

Cold-worked conditions

Cold rolling and drawing lift the strength far above the annealed level because the metastable austenite converts to deformation martensite as it deforms. EN 10151 defines the conditions below for strip and spring material. They are listed here for reference: forgings are supplied solution annealed, not cold worked.

Table 5 — Cold-worked conditions to EN 10151
ConditionTensile strength RmElongation A
+C850850 to 1000 MPa25 % min
+C10001000 to 1150 MPa20 % min
+C11501150 to 1300 MPa15 % min
+C13001300 to 1500 MPa10 % min
+C15001500 to 1700 MPa5 % min
+C17001700 to 1900 MPa2 % min
+C19001900 to 2200 MPa1 % min

Heavy sections. Above about 160 mm diameter the room-temperature values in Table 3 are not automatically guaranteed through thickness. Test location, sampling direction and acceptance values are agreed with the purchaser before forging starts, not after the part is on the test bench.

04

Physical Properties

Table 6 — Physical properties of X10CrNi18-8 (1.4310)
PropertyValue
Density at 20 °C7.9 kg/dm³
Electrical resistivity at 20 °C0.73 Ω·mm²/m
Thermal conductivity at 20 °C15 W/(m·K)
Specific heat capacity at 20 °C500 J/(kg·K)
Linear expansion, 20 to 100 °C16 × 10-6 K-1
Linear expansion, 20 to 200 °C17 × 10-6 K-1
Linear expansion, 20 to 300 °C17 × 10-6 K-1
Linear expansion, 20 to 400 °C18 × 10-6 K-1
Linear expansion, 20 to 500 °C18 × 10-6 K-1
Modulus of elasticity at 200 °C186 GPa
Modulus of elasticity at 400 °C172 GPa
MagnetisabilitySlight when annealed, magnetic after cold forming
05

Forging, Heat Treatment and Machining

Forging

Forgeability is rated good and both open-die forging and drop forging are suitable. Heat slowly to roughly 1150 to 1200 °C and work down to about 900 °C, then cool in air or in water. Some mill datasheets set the finishing floor higher, at 930 °C, and on thin sections that is the safer number to work to. Slow heating matters on heavy sections because thermal conductivity is low at 15 W/(m·K), so a fast ramp puts the surface a long way ahead of the core.

Solution annealing

Optimum properties follow solution annealing between 1000 and 1100 °C with rapid cooling in air or water. Forgings are solution treated after forging as standard. Keep dwell time short in the 450 to 850 °C range: chromium carbide precipitation is the main metallurgical risk with this grade and it is what drives the intergranular corrosion limitation described below.

Machining

Machinability is moderate, and the grade is rarely chosen where heavy machining is the main operation. The high work-hardening rate combined with low thermal conductivity means the tool must stay below the hardened layer left by the previous pass. Use coated carbide, rigid setups, positive uninterrupted cuts and generous coolant. Dwelling or rubbing will glaze the surface and the next pass will struggle.

Table 7 — Indicative turning parameters, solution annealed, Rm 550 to 650 N/mm²
Depth of cutFeed rateCutting speed
6 mm0.5 mm/rev130 m/min
3 mm0.4 mm/rev210 m/min
1 mm0.2 mm/rev250 m/min

Welding

Weldability is good across TIG, arc and laser beam welding. Preheating is not required and post-weld heat treatment is not mandatory, though a solution treatment after welding is advisable where intergranular attack is a concern. Where filler metal is used, a 308L type consumable is recommended and the interpass temperature should stay below 200 °C. Welding cold-worked material destroys the cold-work strength in and around the weld, which is why welded spring components are uncommon in this grade.

06

Corrosion Behaviour and Its Limits

General corrosion resistance is good and polishing improves it noticeably, since surface finish has a strong effect on pitting initiation. Three limits have to be designed around, and all three catch people out.

  1. Not resistant to intergranular corrosion, either in the delivery condition or in the sensitized condition. The carbon content allows chromium carbides to form at the grain boundaries, leaving chromium-depleted zones that corrode preferentially.
  2. Not resistant to seawater or sodium chloride. With a PREN of 16.0 to 23.4, pitting occurs in contact with chlorides. The grade is also susceptible to stress corrosion cracking in chloride and hydroxide environments.
  3. Resistance falls as cold work rises. The strongest cold-formed conditions are also the least corrosion resistant, so strength and corrosion performance have to be traded against each other rather than specified independently.

Against that, the grade performs well in nitric acid, fertiliser compounds, many preservatives and salts, and is resistant to water vapour at room temperature. For sour service, seawater, or any duty requiring certified intergranular corrosion resistance, a stabilised grade such as A182 F321 or A182 F347 is the better starting point, and we can run ASTM A262 or ASTM G28 testing through an accredited laboratory on those grades.

07

Applications

1.4310 suits parts that need high strength after cold work together with reasonable general corrosion resistance. As a spring steel it serves up to 300 °C.

AutomotiveCorrosion-resisting springs, clips, retainers and formed hardware.
Mechanical EngineeringCompression, tension, return, hook and coil springs, spring washers, flexible connectors.
Chemical and Nitrogen PlantValve parts, fittings, pump components, acid tanks and absorption towers.
Food and BeverageProcessing equipment, storage vessels and hygienic-service components.
Heat TransferForged flanges, tube sheets, nozzles and exchanger components.
Rotating EquipmentForged shafts, spindles, gear blanks and rings.
Valves and FittingsBodies, seat rings, stems and blocks for ball, gate, globe and check valves.
ElectricalContact springs and precision formed, polished components.
08

What We Forge in This Grade

Every item is forged from a single piece of steel melted on site. No welding, no casting, no purchased billet of unknown origin. Each is produced against your drawing rather than from a fixed catalogue.

Seamless Rolled RingsRing-rolled from a punched preform on the radial-axial mills, rectangular or contoured section, OD 50 to 6,000 mm.
Forged RingsUpset and punched rings for sections outside the ring-mill envelope.
Forged FlangesWeld neck, blind, slip-on, socket weld, lap joint and orifice to ASME B16.5, B16.47 or EN 1092-1.
Shafts and SpindlesStepped, gear, pinion and eccentric shafts, turned up to 14,000 mm between centres.
Discs and Tube SheetsSolid discs, tube sheets and covers, machined to 5,000 mm diameter, proof-machined for volumetric inspection.
Sleeves and BushingsHollow forged sleeves, bushings and liners, bored to 1,600 mm dia by 10,000 mm deep.
Bars and BlocksForged round, flat and square bars, die blocks and machining blanks.
Valve and Custom PartsBodies, bonnets, seat rings, stems, nozzles, manifolds and near-net shapes.
09

Plant and Route for This Grade

Stainless grades such as 1.4310 take the electric arc, ladle refining and vacuum oxygen decarburisation route. No remelting step is needed, which puts this grade at the shorter end of our lead-time range.

Table 8 — Relevant works capability
StageEquipmentLimit
MeltingElectric arc furnace, ladle furnace, vacuum oxygen decarburisation60 t maximum heat
ForgingHydraulic open-die presses, 6,300 t, 4,000 t and 2,000 t30 t single piece
Ring rollingRadial-axial mills, 6 m, 3 m and 1 mOD 50 to 6,000 mm
Solution annealing14 furnaces, car-bottom and well type8,000 x 2,000 x 2,000 mm; 15 m deep wells
MachiningVertical and horizontal lathes, CNC, deep-hole drilling5,000 mm swing; 14,000 mm length
Minimum orderBy weight, no minimum piece count10 kg
Lead timeNo remelting step required for this grade20 to 60 days

Testing and certification

Chemistry is verified at the furnace by optical emission spectrometry rather than taken from a supplier certificate, because the steel is melted here. Tensile testing runs on 600 kN and 300 kN machines, with ultrasonic inspection to ASTM A388 or EN 10228-3, magnetic particle inspection to ASTM E709 where applicable, and metallographic grain size to ASTM E112. Intergranular corrosion testing to ASTM A262 or G28, which is a common request on this grade given its sensitisation behaviour, is placed with an accredited third-party laboratory and reported alongside the mill certificate.

Table 9 — Documentation
ItemDetail
Class approvalsCCS, BV, DNV, LR, NK
Standard certificateEN 10204 3.1 mill test certificate
Witnessed certificateEN 10204 3.2, witnessed by BV, DNV, LR, SGS, TUV or your own inspector
TraceabilityMelt number through forging, heat treatment and machining to shipment
Supporting recordsHeat-treatment charts, NDT reports, dimensional reports, PMI records
10

Questions We Get Asked

What is X10CrNi18-8 steel?

X10CrNi18-8 is an austenitic chromium-nickel stainless steel with EN material number 1.4310, listed in EN 10088-1, EN 10088-2, EN 10088-3 and EN 10151. It contains 0.05 to 0.15 % C, 16.0 to 19.0 % Cr and 6.0 to 9.5 % Ni. The restricted nickel content leaves the austenite metastable, so the steel work hardens rapidly under cold deformation. That is why the grade is best known as a stainless spring steel.

What is the American equivalent of X10CrNi18-8?

AISI 301 (UNS S30100) and AISI 302 (UNS S30200). Other designations are JIS SUS301 and SUS302, BS 301S21 and 302S26, AFNOR Z11CN17-08 and Z12CN18-09, SS 2331, GOST 12Kh18N9, PN 1H18N9, UNE F-3507, AMS 5516, ISO X9CrNi18-8, and the withdrawn DIN designation X12CrNi17-7. The EN composition band is wider than AISI 301 on both chromium and nickel, so the purchase order should state which standard governs.

Does X10CrNi18-8 contain molybdenum?

No. EN 10088 permits molybdenum only as a residual at maximum 0.80 %, and it is not added deliberately. Where molybdenum is needed for chloride pitting resistance, specify 904L, a 6Mo austenitic grade or a duplex grade instead.

What is the forging temperature of X10CrNi18-8 / 1.4310?

Heat slowly to roughly 1150 to 1200 °C and forge down to about 900 °C, then cool in air or water. Some mill datasheets set the finishing floor higher, at 930 °C. Open-die forging and drop forging are both suitable, and solution annealing at 1000 to 1100 °C follows.

Is X10CrNi18-8 magnetic?

Only slightly magnetisable when solution annealed. Cold forming turns part of the metastable austenite into deformation martensite, after which the material responds to a magnet. This is normal for the grade and is not evidence of the wrong material being supplied.

Is X10CrNi18-8 resistant to intergranular corrosion?

No, neither in the delivery condition nor in the sensitized condition. Chromium carbides form at the grain boundaries and leave chromium-depleted zones. Limit time in the sensitising range during fabrication, and apply a solution treatment after welding or hot forming.

Can X10CrNi18-8 be welded?

Yes. Weldability is good across TIG, arc and laser beam welding. Preheating is not needed and post-weld heat treatment is not mandatory. Where filler is used, a 308L type consumable is recommended with interpass temperature below 200 °C. Welding cold-worked parts removes the cold-work strength locally.

Is X10CrNi18-8 suitable for seawater?

No. With a PREN of 16.0 to 23.4 the grade is not resistant to seawater or sodium chloride, and pitting occurs in contact with chlorides. It is also susceptible to stress corrosion cracking in chloride and hydroxide environments.

Who supplies open-die forgings in X10CrNi18-8?

Jiangyin Jiangnan Metal Co., Ltd., an integrated melting works and open-die forging factory at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Stainless grades are melted in-house through the electric arc furnace, ladle furnace and vacuum oxygen decarburisation route. Rings roll to 6,000 mm outside diameter and single pieces reach 30 tonnes. Minimum order is 10 kg and lead time runs 20 to 60 days. Telephone +86 189 2135 9659, email sales@steelforgepieces.com.

What is the minimum order quantity?

10 kg, with no minimum piece count. A single small part is quotable and so is a one-off large ring. Very small parts are grouped into a batch to share furnace and setup time, so quantity still affects the unit price even though it does not affect whether we can take the job.

What do you need in order to quote?

Six things: the grade or specification, the dimensions or a drawing, the quantity and expected repeat volume, the delivery condition, the heat treatment and testing requirements, and the certification level plus destination port. Sending all six in the first email usually gets a price back within two working days.

Request a Quotation

Send a drawing or dimensions and we will quote forged weight, price and lead time for X10CrNi18-8 rings, flanges, shafts, discs and bars. Customer audits, pre-shipment inspection and third-party witness testing are welcome; please arrange visits by email in advance so an English-speaking engineer is available.

Company
Jiangyin Jiangnan Metal Co., Ltd.
Plant
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone, WhatsApp, WeChat
+86 189 2135 9659
Hours
Monday to Saturday, 08:00 to 17:30 China Standard Time, UTC+8
Minimum order
10 kg, no minimum piece count

Email the works