DATASHEET UNS S44400 / AISI 444 / EN 1.4521 / SUS444 REV 2026-10-09 TEL +86 189 2135 9659   EMAIL sales@steelforgepieces.com
Jiangnan Metal Melting works · Open-die forge · Ring mill Request quote

Ferritic stainless steel · Dual stabilised 18Cr-2Mo

UNS S44400 Forgings Forged bars, seamless rolled rings, discs, sleeves and machined components in AISI 444 / EN 1.4521 / SUS444

UNS S44400 is a low-carbon, low-nitrogen ferritic stainless steel of roughly 17.5 to 19.5 percent chromium and 1.75 to 2.50 percent molybdenum, dual stabilised with titanium and niobium. It gives pitting and crevice corrosion resistance better than most ferritic stainless steels and some austenitic grades, matches Type 304 in many corrosion environments, and resists chloride stress corrosion cracking better than both Type 304 and Type 316.

Jiangyin Jiangnan Metal melts this grade in its own furnaces and forges it on site. The electric arc furnace, ladle furnace and vacuum oxygen decarburisation route holds the low carbon and controlled nitrogen the grade depends on, and the certificate traces a finished part back to its melt number rather than to a purchased billet.

Grade summaryS44400
UNS
S44400
Also
AISI 444 · EN 1.4521 · X2CrMoTi18-2 · SUS444
Structure
Ferritic, Ti and Nb dual stabilised
Cr / Mo
18 % / 2 %
PREN
25
Forging
1050 to 750 C
Anneal
750 to 900 C
Max ring
6,000 mm OD
Max piece
30,000 kg
Min order
10 kg, no minimum piece count
Certificate
EN 10204 3.1, 3.2 on request
01

What the grade is for

Type 444 was developed to bring 300-series corrosion performance to a ferritic steel without depending on nickel. Carbon sits at 0.025 percent maximum and nitrogen at 0.035 percent maximum, and titanium and niobium are added together so chromium carbides cannot precipitate at grain boundaries after welding or hot work.

The practical result is a steel that resists pitting and crevice attack better than most ferritics, stays oxidation and creep resistant at elevated temperature, and holds up against chloride stress corrosion cracking. That last property is the reason it exists. Chloride SCC is the failure mode that most often retires 304 and 316 parts from hot chloride-bearing water service, and it is not a defect of manufacture that a better supplier can engineer away.

Against Type 304 the grade also expands less with temperature and conducts heat better, which is why it appears in heat exchanger tubing, hot water tanks and automotive exhaust work. Published corrosion data shows good behaviour in moderately severe environments containing chlorides and the organic acids found in foods and beverages, with satisfactory resistance to dilute sulfuric acid and to highly concentrated sodium hydroxide. For immersed service the grade is generally considered suitable below roughly 200 ppm chloride, with a tighter limit for hot water.

For forged parts there are three things to plan around. The steel hot works predictably but coarsens if soaked too hot, so soak and finish temperatures matter. It must be annealed before machining or the part will move afterwards. And welding needs more care than a 409, which is covered in section 05.

02

Equivalent designations

The same material is sold under at least eight national designations. Chemistry windows are not identical, so the ordering standard governs, not the trade name.

UNS S44400 cross-reference
Standard or regionDesignation
UNS, USAS44400, closely related S44401
AISI and ASTM, USAType 444, TP444 for tubing, 18Cr-2Mo
EN, Europe1.4521, X2CrMoTi18-2
JIS, JapanSUS444
GB/T, China019Cr19Mo2NbTi, 00Cr18Mo2
NF, FranceZ3CDT18-02, Z3CDFT18-02
SS, Sweden2326
UNE, SpainF3123

Source: Virgamet 1.4521 / X2CrMoTi18-2 cross-reference table.

Do not confuse

Type 444 is not ASTM A182 F44. Despite the similar number, A182 F44 is UNS S31254, a 6Mo austenitic stainless steel, and is a different material with different welding, machining and corrosion behaviour. Both are forged here. They are not substitutes for one another.

03

Chemical composition

Weight percent, balance iron. Where a cell reads not specified, that standard sets no limit for the element and it is controlled by agreement instead.

Composition limits by ordering standard
ElementASTM A276 / A276M, S44400EN 1.4521JIS SUS444
Carbon, C0.025 max0.025 max0.025 max
Silicon, Si1.00 max1.0 max1.0 max
Manganese, Mn1.00 max1.0 max1.0 max
Phosphorus, P0.040 max0.040 max0.040 max
Sulfur, S0.030 max0.015 max0.030 max
Chromium, Cr17.5 to 19.517.0 to 20.017.0 to 20.0
Molybdenum, Mo1.75 to 2.501.8 to 2.51.75 to 2.50
Nickel, Ni1.00 maxnot specifiednot specified
Nitrogen, N0.035 max0.03 max0.025 max
Titanium, TiTi plus Nb: 0.20 plus 4 x (C+N) minimum, 0.80 maximum0.15 to 0.80not specified
Niobium, Nbnot specifiednot specified
Iron, FeBalance

Sources: Ferrobend ASTM A276/A276M UNS S44400 datasheet; Virgamet EN 1.4521 and SUS444 comparison; Cleveland-Cliffs Type 444 product data sheet for the titanium and niobium stabilisation rule.

Correction to a figure in circulation

A nitrogen limit of 0.1 percent is quoted for this grade on a number of trading sites, including an earlier revision of this page. It matches no governing standard. ASTM A276 allows 0.035 percent maximum and EN 1.4521 allows 0.03 percent maximum. Nitrogen matters here because this is a stabilised ferritic grade: the required titanium and niobium addition is calculated from carbon plus nitrogen, so an inflated nitrogen figure silently changes the stabilisation requirement. Chemistry on our certificates is reported against the ordering standard and verified at the furnace by optical emission spectrometry to ASTM E415, with carbon and sulfur by infrared analysis to ASTM E1019.

04

Mechanical and physical properties

Room temperature mechanical requirements and typical values
PropertyA276 hot finished barA276 cold finished barTypical, flat product
Tensile strength415 MPa (60 ksi) min415 MPa (60 ksi) min515 MPa (75 ksi)
Yield strength, 0.2 %310 MPa (45 ksi) min310 MPa (45 ksi) min360 MPa (52 ksi)
Elongation, 2 in or 4D20 % min16 % min30 %
Reduction of area45 % min45 % minnot stated
Hardness217 HBW max217 HBW maxHRB 85

Sources: Ferrobend ASTM A276/A276M UNS S44400; Cleveland-Cliffs 444 Stainless product data sheet for typical flat product values.

Under the European standard, annealed 1.4521 cold rolled strip is specified at 420 to 640 MPa tensile with 300 MPa minimum yield, 20 percent minimum elongation and hardness below 185 HB, while hot rolled plate is 420 to 620 MPa tensile with 280 MPa minimum yield. Proof strength falls from about 294 MPa at 50 C to about 200 MPa at 400 C, which is the figure to design against for warm service rather than the room temperature value.

Physical properties at or near room temperature
PropertyValueReference
Density7.75 g/cm3 (0.28 lb/in3); 7.73 g/cm3 for 1.4521Cleveland-Cliffs / Virgamet
Thermal conductivity at 100 C26.8 W/m-K (15.5 BTU/hr-ft-F)Cleveland-Cliffs
Thermal expansion, 0 to 100 C11.0 micrometre/m-KCleveland-Cliffs
Specific heat, 0 to 100 C0.427 kJ/kg-KCleveland-Cliffs
Electrical resistivity at 21 C57 micro-ohm-cmCleveland-Cliffs
Modulus of elasticity220 GPa for 1.4521; 200 GPa reported for AISI 444Virgamet / AZoM
Poisson ratio0.27 to 0.30AZoM
PREN25Virgamet
05

Forging, heat treatment and welding

Published working parameters for the equivalent 1.4521 grade: forging and hot rolling 1050 to 750 C with water, air or gas cooling, annealing 750 to 900 C with air or gas cooling, furnace cooling only in special cases.

Ferritic stainless steels have no phase transformation to refine a coarse grain, so an overheated soak cannot be corrected later by heat treatment the way it can in a quenched and tempered alloy steel. Soak temperature and finish forging temperature are therefore both recorded on the heat treatment chart that ships with the forging. Annealing is carried out before rough machining so the part is dimensionally settled before metal comes off it.

Heat treatment runs on site across 14 furnaces, including car-bottom furnaces with working chambers up to 8,000 x 2,000 x 2,000 mm and two 15 m deep well-type furnaces for long shafts. No heat treatment step is subcontracted.

Welding

Type 444 welds by the common fusion and resistance methods but is less forgiving than Type 409. The higher chromium plus the molybdenum and niobium mean low heat input and few discontinuities are needed, and slight pre-warming is sometimes used to avoid brittle fracture during forming that follows welding, particularly in cold weather. Where filler metal is required, AWS E/ER 316L is the usual choice. Note that our forgings are made from a single piece of steel, with no welding in the part itself.

06

Forged product forms and size envelope

Every item below is forged from one piece of steel melted on site. No casting, no welded fabrication, no purchased billet of unknown origin.

Available forms in S44400 and the equipment that sets the limit
FormShapesSize limit and what sets it
Seamless rolled rings Rectangular and contoured section, flange blanks, gear ring blanks OD 50 to 6,000 mm. 6 m radial-axial mill, with 3 m and 1 m mills below it and an upset-and-punch route for the smallest sizes
Forged rings Upset and punched rings, retaining rings, valve seat rings Sections outside the ring mill envelope, worked on the 6,300 t, 4,000 t and 2,000 t presses
Forged bars Round, square, rectangular, flat and hexagon Turned to 1,800 mm dia x 8,000 mm, or 1,600 mm dia x 14,000 mm on the C61160 lathe
Hollows and sleeves Hollow bar, sleeve, bush, cylinder, shell, hub, housing, heavy wall pipe section Bored to 1,600 mm dia x 10,000 mm on the CNC deep-hole drilling machine
Discs and blocks Solid discs, tube sheets, covers, blocks, plates Machined to 5,000 mm diameter on the vertical lathe, supplied proof-machined for volumetric inspection
Single piece weight Any of the above Up to 30,000 kg, set by the 60 t maximum heat and the 6,300 t press

Standards for ordering and certification

  • ASTM A276 / A276M — hot and cold finished stainless bars in rounds, squares, hexagons and hot rolled or extruded shapes, including S44400. The usual ordering standard for bar stock.
  • ASTM A479 / A479M — stainless steel bars and shapes for boilers and other pressure vessels, which lists S44400 among the ferritic grades. Use this one where ASME Section VIII applies.
  • ASTM A240 and ASME SA240 — plate, sheet and strip, under which Type 444 flat product is supplied.
  • ASTM A268 and ASME SA268 — seamless and welded ferritic and martensitic stainless tubing for general service, grade TP444.
  • ASTM A815 / A815M — wrought ferritic, ferritic-austenitic and martensitic stainless piping fittings.
  • ASTM A959 and SAE J405 — composition listings for wrought stainless grades, used for cross-reference on certificates.

Scopes taken from the published ASTM specification summaries. The applicable edition is fixed at order placement.

07

Testing and certification

The works holds CCS, BV, DNV, LR and NK approvals and runs its own laboratory. Because the steel is melted here, chemistry is verified at the furnace rather than taken from a supplier certificate.

Testing available in house for S44400 forgings
DisciplineEquipmentStandard
Chemical analysisMobile optical emission spectrometer, SPECTROTEST TXC25ASTM E415
Carbon and sulfurInfrared analyser, HIR-9440DASTM E1019
Alloy verificationHandheld analyser, X-Mwt3000TXPositive material identification
Tensile600 kN WE-600B and 300 kN WDW-300ASTM A370, ISO 6892
HardnessLeeb tester TH140ASTM A956, converted per ASTM E140
UltrasonicPXUT-3300, USM35XS, CTS-22ASTM A388, EN 10228-3
Magnetic particleCYE-3AASTM E709
Grain sizeXJP-6A microscope with specimen preparationASTM E112
Placed with an accredited third-party laboratory

Intergranular corrosion testing to ASTM A262 or ASTM G28 and pitting resistance to ASTM G48 are not run in house. For a stabilised ferritic grade like S44400 these are the tests most often called for, so flag them at enquiry stage: the report is issued by the outside laboratory alongside our mill certificate, and the scheduling affects the delivery date. Standard documentation is EN 10204 3.1. EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector is available on request.

08

Questions

What is UNS S44400 stainless steel?

Type 444, an 18Cr-2Mo low carbon, low nitrogen ferritic stainless steel dual stabilised with titanium and niobium, with about 17.5 to 19.5 percent chromium, 1.75 to 2.50 percent molybdenum and carbon at 0.025 percent maximum. Stabilisation prevents sensitisation; the molybdenum provides pitting and crevice corrosion resistance better than most ferritic stainless steels and some austenitic ones.

Is S44400 the same as AISI 444, 1.4521 and SUS444?

They are national designations for essentially the same steel. The limits differ slightly: EN allows chromium 17.0 to 20.0 percent while ASTM A276 narrows it to 17.5 to 19.5 percent, and the sulfur and nitrogen caps differ too. State the ordering standard on the purchase order and the certificate will be written against it.

Why specify Type 444 instead of 304 or 316?

It matches Type 304 in many corrosion environments, expands less with temperature, conducts heat better, and resists chloride stress corrosion cracking better than both 304 and 316. Being essentially nickel free, its cost is less tied to the nickel price. In exchange you accept lower toughness in heavy sections and tighter welding practice.

What are the forging and annealing temperatures?

Forging 1050 to 750 C, annealing 750 to 900 C with air or gas cooling, furnace cooling only in special cases. Because a ferritic grade has no transformation to refine coarsened grain, soak and finish forging temperatures are recorded on the heat treatment chart supplied with the part.

How large a S44400 ring or forging can you make?

Rings roll to 6,000 mm outside diameter on the 6 m radial-axial mill, down to 50 mm by the upset and punch route. The heaviest single forging is 30 tonnes on the 6,300 t press. Machining reaches 5,000 mm swing on the vertical lathe, 14 m between centres on the horizontal lathe, and 1,600 mm by 10,000 mm on the deep-hole borer.

Which filler metal for welding Type 444?

AWS E/ER 316L is the filler most often specified. Keep heat input low, avoid discontinuities, and consider slight pre-warming before any forming that follows welding.

Minimum order and lead time?

10 kg minimum, no minimum piece count, so a single prototype is quotable. Lead time 20 to 60 days. S44400 is a standard stainless grade needing no remelting step, so it sits at the lower end of that range unless witnessed inspection or outside laboratory corrosion testing has to be scheduled into it.

What do you need in order to quote?

Six items: the grade or specification, dimensions or a drawing in PDF, DWG, DXF or STEP, the quantity and expected repeat volume, the delivery condition (as forged, proof machined or finish machined), the heat treatment and testing requirements, and the certification type with destination port. Sending all six in the first email usually gets a price back within two working days.

09

Request a quotation

Send a drawing or a written specification for UNS S44400 bars, rings, discs, sleeves or machined components. Quotations are normally returned within two working days. Customer audits, pre-shipment inspection and third-party witness testing are welcome; arrange visits by email in advance so an English-speaking engineer is available.

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Business hours: Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8)

10

Related grades

Grades frequently compared with S44400 or specified alongside it on the same enquiry.

Technical data on this page is compiled from published mill and standards documentation, including the Cleveland-Cliffs Type 444 product data sheet, the Ferrobend ASTM A276/A276M S44400 summary, the Virgamet EN 1.4521 datasheet and the AZoM Grade 444 datasheet. It is given for guidance. Values for a specific order are governed by the ordering standard and by the mill certificate supplied with the goods. Plant capability figures are those of Jiangyin Jiangnan Metal Co., Ltd.