Grade data sheet UNS S30100 / Type 301 Revision 2026-10-05 Markdown copy: UNS-S30100.md +86 189 2135 9659
Jiangyin Jiangnan Metal Melting works and open-die forge, Jiangyin, China Request quote

Austenitic stainless steel, 17 Cr / 7 Ni

UNS S30100 Type 301 grade data, forging practice and what we make from it

UNS S30100, designated Type 301 in the AISI and ASTM systems, is an austenitic chromium-nickel stainless steel with a nominal 17 percent chromium and 7 percent nickel and a carbon ceiling of 0.15 percent. It carries no molybdenum.

The nickel content is lean by design, which leaves the austenite metastable and gives the grade its defining property: a very high work-hardening rate. Cold rolling lifts tensile strength from a 515 MPa annealed minimum to a 1276 MPa minimum at full hard, which is why the grade is sold by temper rather than as a single property set.

Because that strength comes from rolling, S30100 is standardised as a flat-rolled product in ASTM A240 and ASTM A666 and is not a listed grade in the stainless forging specifications. Section 01 sets out what that means when you order a forging, and what we supply instead.

Grade summaryS30100
UNS
S30100
Type
301, austenitic Cr-Ni
Nominal
17 Cr / 7 Ni, 0.15 C max
Molybdenum
None
Annealed min
515 MPa UTS, 205 MPa YS, 40 percent
Full hard min
1276 MPa UTS, 965 MPa YS
Forge
1093 to 1204 C, finish 927 C
Anneal
1010 to 1121 C, cool fast
Specified in
ASTM A240, ASTM A666
Equivalents
EN 1.4310, JIS SUS 301, GB 12Cr17Ni7
01

Specification status before you order

This is the first thing to settle on an S30100 enquiry, and it is where most published grade pages go wrong. Type 301 earns its place in engineering through cold rolling, so the standards that define it are flat-product standards.

Table 1. Where S30100 is and is not specified
SpecificationScopeS30100 listed
ASTM A666/A666MAnnealed or cold-worked austenitic stainless steel sheet, strip, plate and flat barYes. Type 301 is the grade this standard is best known for
ASTM A240/A240MChromium and chromium-nickel plate, sheet and strip for pressure vessels and general applicationsYes
ASTM A473Stainless steel forgings for general use and for low or high temperature serviceNo. The austenitic list runs S20100, S20200, S20500, S21900, S21904, S28200, S30200, S30215, S30300, S30400 and upward. S30100 is absent
ASTM A182/A182MForged or rolled flanges, fittings, valves and parts for high temperature serviceNo. The austenitic family is F304, F304L, F316, F316L, F317, F317L, F321 and F347 type grades

Sources: ASTM A473-19 Table 1, chemical requirements. ASTM A666/A666M title and scope. ATI 301 technical data sheet, which gives the composition as represented by ASTM A240 and A666.

What this means in practice

Three honest routes exist when a drawing calls for a 301 forging. Forge to S30100 chemistry with mechanical acceptance agreed in the purchase order rather than quoted from a forging standard, which we can do and certify. Substitute Type 304 or 304L, a listed grade in both A473 and A182, trading work-hardening rate for better ductility and weldability. Or substitute Type 316 or 316L where corrosion resistance governs. Send the drawing and we will set out cost and lead time against each option rather than quote the grade blind.

02

Chemical composition

Table 2. Composition limits, weight percent, maximum unless a range is shown
ElementLimitNote
Carbon, C0.15 maxHigh for an austenitic grade. This is what drives the sensitisation risk on welding
Chromium, Cr16.00 to 18.00Nominal 17
Nickel, Ni6.00 to 8.00Nominal 7, lean by design, which keeps the austenite metastable
Manganese, Mn2.00 maxNot restricted further
Silicon, Si0.75 maxThe ATI data sheet and A240 give 0.75 max. Some grade tables show 1.00 max, so confirm against your specification edition
Phosphorus, P0.045 maxNot restricted further
Sulfur, S0.030 maxNot restricted further
Nitrogen, N0.10 maxRaising nitrogen above this is the basis of the 301LN variant
Molybdenum, MoNot specifiedNot an alloying addition in this grade
Iron, FeBalanceNot restricted further

Sources: ATI 301 technical data sheet, UNS S30100. AZoM grade 301 composition table covering ASTM A666, JIS G4305 for 301L and EN 10088-2 grade 1.4318 for 301LN.

Low carbon and nitrogen variants

Two variants are often confused with the base grade. 301L cuts carbon to 0.03 percent maximum with nitrogen to 0.20 percent maximum and is covered by JIS G4305, chosen where ductility and as-welded corrosion behaviour matter. 301LN is EN 10088-2 grade 1.4318, with 0.10 to 0.20 percent nitrogen and 16.5 to 18.5 percent chromium, and work-hardens faster than standard 301. Of the three, only plain 301 is specified in ASTM A666.

03

Mechanical properties by temper

Specification minimums for flat product. A forging supplied in the annealed condition is assessed against the annealed row, with acceptance values fixed in the order.

Table 3. Minimum room-temperature properties, ASTM A240 and A666
TemperTensile strength minYield 0.2 percent offset minElongation in 50 mm min
Annealed515 MPa / 75 ksi205 MPa / 30 ksi40 percent
1/16 hard620 MPa310 MPa40 percent
1/8 hard690 MPa380 MPa40 percent
1/4 hard862 MPa / 125 ksi517 MPa / 75 ksi25 percent
1/2 hard1034 MPa / 150 ksi758 MPa / 110 ksi18 percent
3/4 hard1207 MPa / 175 ksi931 MPa / 135 ksi12 percent
Full hard1276 MPa / 185 ksi965 MPa / 140 ksi9 percent

Sources: ATI 301 technical data sheet, minimum room-temperature mechanical properties per ASTM A240 and A666. AZoM grade 301 temper table, which gives the same values from 1/16 hard through full hard. Hardness varies with temper and is reported on the test certificate rather than quoted here.

A data conflict worth knowing about

Some published tables list annealed 301 as 758 MPa tensile, 276 MPa yield and 60 percent elongation. Those are typical values rather than specification minimums. ATI gives typical annealed room-temperature figures of about 724 MPa tensile, 276 MPa yield and 55 to 60 percent elongation, which agree closely. For acceptance testing and design allowables, use the 515, 205 and 40 percent figures from Table 3.

Low temperature and fatigue

Annealed 301 holds Charpy V-notch energy of roughly 150 J, or 110 ft-lb, from plus 23 C down to minus 196 C with no ductile to brittle transition, which is the reason annealed austenitic grades are used in cryogenic work. Tensile strength climbs steeply as temperature drops: typical annealed material moves from about 724 MPa at room temperature to about 1896 MPa at minus 196 C, with elongation still near 30 percent. Endurance limit of annealed material is 30 to 45 percent of tensile strength, around 241 MPa, rising to roughly 552 MPa at full hard.

04

Physical properties

Table 4. Representative physical properties, annealed condition
PropertyValue
Density7.88 to 8.03 g/cm3, 0.29 lb/in3
Modulus of elasticity in tension193 GPa, 28 million psi. Lower in the cold-worked condition
Melting range1399 to 1421 C, 2550 to 2590 F
Mean thermal expansion, 20 to 100 C16.6 to 16.9 micrometre per metre per C
Mean thermal expansion, 20 to 500 C18.2 to 18.6 micrometre per metre per C
Thermal conductivity at 100 C16.2 to 16.3 W/m.K
Thermal conductivity at 500 C21.4 W/m.K
Specific heat, 0 to 100 C500 J/kg.K
Electrical resistivity at 20 C695 to 720 nanoohm.metre, 72 microohm.cm
Magnetic permeability, properly annealed1.02 maximum at 200 H, effectively non-magnetic
Magnetic permeability, cold workedRises with the amount of deformation as martensite forms

Sources: ATI 301 technical data sheet, physical properties and magnetic permeability. AZoM grade 301 physical property table. Expansion is higher than many other metals, which should be allowed for in mixed-material assemblies.

05

Forging and heat treatment

Forging range

Start at 1093 to 1204 C, or 2000 to 2200 F. Finish at about 927 C, or 1700 F. Reheat rather than push the finish temperature down.

Solution anneal

1010 to 1121 C, or 1850 to 2050 F, then cool rapidly through the carbide precipitation range. Water quench heavy sections. Air cooling suits thin sections.

Stress relief after cold work

371 to 538 C, or 700 to 1000 F, held from five minutes to five hours, which evens out properties. Lower temperature and shorter time limit carbide precipitation.

No hardening by heat treatment

Strength in this grade comes from cold work, not from quench hardening. Thermal hardening does not apply.

Two behaviours govern what happens downstream. Strain-hardened austenite partly transforms to martensite, so a part that is non-magnetic as forged and annealed can turn noticeably magnetic after cold sizing or roll forming. Separately, time in the 427 to 816 C band, or 800 to 1500 F, precipitates carbides at the grain boundaries. That single mechanism sits behind both sensitisation and the welding limits in section 06.

The same rapid work hardening makes machining and cold shaping harder than on Type 304, so tooling, feeds and speeds should be set for a work-hardening austenitic grade rather than carried over from a free-machining steel.

06

Corrosion, oxidation and welding

Published assessments differ in emphasis here, and both views are useful. AZoM puts the corrosion resistance of 301 on a par with Type 304, good in mildly corrosive conditions at ambient temperature. ATI is more guarded, stating that while 301 resists a range of corrosive media its corrosion properties are not as good as the 18-8 chromium-nickel steels, and that susceptibility to carbide precipitation during welding restricts its use in favour of 304 or 304L.

Carbon reconciles the two positions. At up to 0.15 percent carbon, 301 is far more prone to sensitisation than 304L, so the gap between the grades widens sharply once a part has been welded or held in the sensitising range. In the annealed, unwelded condition the two behave much alike.

Table 5. Service and fabrication limits
ConditionGuidance
Oxidation resistanceGood to about 840 C. At 871 C weight gain reaches 10 mg per square cm in 1000 hours, so the grade is not suggested at or above 871 C. One published data sheet extends intermittent service to 840 C and continuous service to 900 C. Treat 840 C as the conservative ceiling
Elevated temperature designShort-time high-temperature tensile data supports design only to roughly 370 to 425 C, or 700 to 800 F. Above that, design on creep and stress-rupture data. There is no significant creep advantage over other 18-8 grades
WeldingSuitable for the standard methods. Recommended filler is 308L. Weldments in plain 301 should be annealed afterwards for maximum corrosion resistance, while 301L and 301LN do not require post-weld annealing
Spot weldingWidely used to assemble cold-rolled 301 components. The short cycle does not materially reduce component strength
Trade-off on post-weld annealAnnealing removes the strength gained by cold rolling. If a cold-worked temper was specified for strength, the joint design has to avoid needing a full solution anneal

Sources: ATI 301 technical data sheet, corrosion resistance, oxidation, elevated-temperature design and heat treatment sections. AZoM grade 301 corrosion, heat resistance and welding sections.

07

Equivalents and alternatives

Table 6. Approximate international designations for Type 301
SystemDesignation
UNSS30100
AISI and ASTMType 301
EN1.4310, X10CrNi18-8
Former British BS301S21
Swedish SS2331
JISSUS 301
GB12Cr17Ni7, formerly 1Cr17Ni7

Sources: AZoM grade 301 grade comparison table. Published 1.4310 equivalence tables listing AISI 301, JIS SUS301 and GB 12Cr17Ni7. These are functionally similar grades, not exact equals. Check the governing specification before substituting.

Where a substitution is open, the choice is straightforward. Type 304 suits parts that can accept a lower work-hardening rate and benefit from better forming ductility, which covers most forgings. Type 316 suits parts where corrosion resistance decides the material and the lower work-hardening rate can be designed around.

08

Where Type 301 is actually used

The grade earns its applications through high cold-worked strength, retained ductility and a bright surface, almost always in sheet, strip or formed section. It is supplied as cold rolled strip, sheet and plate.

Rail and transit

Railway and subway car structural components, commonly roll formed, brake pressed or stretch formed to profile.

Road transport and airframe

Airframe sections, highway trailer components, truck and trailer bodies.

Automotive trim

Mouldings and trim, wheel covers, wiper blade clips and holders.

Springs and clips

Springs, hose clamps and stove element clips, in tempers from three-quarter to full hard where wear resistance and spring action are wanted with simple form designs.

Architectural

Curtain walls, screen frames, roof drainage systems and decorative structural work.

Equipment

Conveyor belts and kitchen equipment.

Sources: ATI 301 technical data sheet applications section. AZoM grade 301 applications list. Atlas Steels 301, 301L and 301LN grade data sheet.

Duties this grade does not cover

Type 301 is sometimes listed against pressure vessels, shell and tube exchangers, subsea and deepwater production systems, fluid catalytic cracking units, polythionic acid service, wellheads and Christmas trees. Those duties belong to other grades, typically 321 and 347H, F316L, or duplex and super duplex such as F51, F53 and F55, and are not supported for S30100. If your enquiry sits in that territory, ask us for the right grade rather than this one.

09

What we forge in S30100

Jiangyin Jiangnan Metal melts its own steel. Carbon, alloy, stainless and duplex grades run through the electric arc furnace, the ladle furnace and vacuum oxygen decarburisation, then move through the presses, the ring mill, 14 heat-treatment furnaces and the machine shop without leaving the site. Certification traces a part back to its melt number rather than stopping at a purchased billet.

Table 7. Forms and working envelope
FormEnvelopeSet by
Seamless rolled ringsOD 50 mm to 6,000 mm6 m radial-axial ring mill, with an upset and punch route below ring-mill range
Forged rings and sleevesSections outside the ring-mill envelope6,300 t, 4,000 t and 2,000 t open-die presses
Discs, tube sheets, blocksUp to 5,000 mm machined diameter5,000 mm vertical turning lathe
Shafts and spindlesUp to 14,000 mm turned lengthC61160 horizontal lathe, 15 m well furnace for vertical quench
Bored cylinders, hollow shaftsUp to 1,600 mm diameter by 10,000 mmCNC deep-hole drilling machine
Round bar, blocks, blanksSingle piece to 30,000 kg60 t maximum heat, 6,300 t press

Inspection and certification

Ultrasonic examination is carried out to EN 10228-3, SEP 1921 or ASTM A388 as the order requires. Certification is issued to EN 10204 3.1, or 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector. The works holds CCS, BV, DNV, LR and NK classification society approvals and runs its own laboratory for chemistry, tensile, impact, ultrasonic, magnetic particle and metallographic testing. Where a part is nominally a flange, fitting or valve component for pressure service, we will normally recommend an A182 listed grade for the reasons in section 01.

What to send with an enquiry

A quote moves fastest with the drawing or finished dimensions including machining allowance, the quantity, the required condition or temper, the acceptance standard the forging is to be certified against, any non-destructive testing requirement, and the certification level and destination port. If you have a preferred melting and refining route, state it and we will confirm what we can supply rather than assume.

10

Request a quotation

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town,
Jiangyin City, Jiangsu Province, China

+86 189 2135 9659 sales@steelforgepieces.com

Telephone, WhatsApp and WeChat on the same number. Business hours Monday to Saturday, 08:00 to 17:30 China Standard Time, UTC+8.

Commercial terms

  • Minimum order 10 kg, no minimum piece count
  • Lead time 20 to 60 days from order confirmation
  • Price quoted against drawing, weight and quantity
  • Steel melted and forged in one works, operating since 1997
  • 460 staff, including 9 senior and 32 intermediate engineers
  • CCS, BV, DNV, LR and NK approvals
  • Exports to North America, Europe, the Middle East and Asia-Pacific
11

Questions we are asked about this grade

Does UNS S30100 contain molybdenum?

No. It is a plain chromium-nickel austenitic stainless steel, nominally 17 percent chromium and 7 percent nickel, and the composition limits in ASTM A240 and A666 carry no molybdenum addition. Data describing S30100 as molybdenum-bearing or vacuum remelted belongs to a different grade, usually a 316 type or a precipitation-hardening grade.

Is UNS S30100 an ASTM A182 grade?

No. The A182 austenitic family covers F304, F304L, F316, F316L, F317, F317L, F321 and F347 type grades. S30100 is specified for plate, sheet, strip and flat bar in ASTM A240 and A666, and it is also absent from the chemical requirements table of ASTM A473, the stainless forgings specification.

What are the annealed minimum properties?

515 MPa or 75 ksi tensile, 205 MPa or 30 ksi yield at 0.2 percent offset, and 40 percent elongation in 50 mm, per ASTM A240 and A666. Typical annealed values run higher, around 724 MPa, 276 MPa and 55 to 60 percent.

What is the forging temperature range?

Start at 1093 to 1204 C, finish around 927 C, then solution anneal at 1010 to 1121 C with rapid cooling to hold carbides in solution.

Is Type 301 magnetic?

Properly annealed material is austenitic and effectively non-magnetic, with permeability of 1.02 maximum at 200 H. Cold work forms martensite and permeability rises with the amount of deformation.

Can it be used for high-temperature strength?

Only within limits. Short-time elevated tensile data supports design to roughly 370 to 425 C. Above that, creep and stress-rupture data govern, and 301 holds no meaningful creep advantage over other 18-8 grades. Oxidation resistance is good to about 840 C and the grade is not suggested at or above 871 C.

What filler metal is used to weld it?

308L. Weldments in plain 301 should be annealed afterwards for maximum corrosion resistance. The 301L and 301LN variants avoid that requirement.

Which grade replaces 301 for forgings?

Type 304 or 304L in most cases, because it is listed in both ASTM A473 and ASTM A182, work-hardens less and welds more easily. Type 316 or 316L where corrosion resistance governs.

Reviewed 5 October 2026 by technical sales, Jiangyin Jiangnan Metal Co., Ltd. Data compiled from the ATI 301 technical data sheet for UNS S30100, the AZoM grade 301 data sheet, the Atlas Steels 301, 301L and 301LN data sheet, ASTM A473-19 and the published titles and scopes of ASTM A666/A666M and A240/A240M. Figures are for guidance. They are not design allowables and do not replace the governing specification edition or your own engineering review. A plain-text copy of this page is published at /Stainless-Steel/UNS-S30100.md.