Material data sheet · Austenitic stainless steel
UNS S24000 Forgings ASTM XM-29 · Nitronic 33 · 18-3-Mn — rings, flanges, bars, shafts and discs, melted and forged in one works
S24000 is the nitrogen-strengthened, high-manganese stainless that buyers reach for when a part has to be strong, stay non-magnetic after machining, and survive cold service. We melt it, forge it and heat treat it on one site in Jiangyin.
UNS S24000 contains 17 to 19 % chromium, 11.5 to 14.5 % manganese, 2.25 to 3.75 % nickel and 0.20 to 0.40 % nitrogen, with carbon capped at 0.08 %. Manganese and nitrogen hold the austenite in place of nickel. Nitrogen in solid solution lifts annealed yield strength to roughly twice that of Type 304, while the alloy keeps good ductility and toughness down to cryogenic temperatures and holds low magnetic permeability even after severe cold working. ASTM calls the grade XM-29; the mill trade name is Nitronic 33.
There is no molybdenum in S24000. It is a strength, non-magnetic and low-temperature grade, not a seawater or acid grade. Normal forged uses are non-magnetic rings and containment rings, cryogenic valve and vessel parts, pump and valve components, rotating parts such as fans, and heavily loaded structural parts. XM-29 is also a recognised stainless reinforcing bar grade under ASTM A955.
Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, forges S24000 rings, rolled rings, flanges, bars, shafts, discs, tube sheets, sleeves and bushings to drawing. Rings run to 6,000 mm outside diameter, single pieces to 30 tonnes, minimum order 10 kg, lead time 20 to 60 days. Telephone +86 189 2135 9659, email sales@steelforgepieces.com.
- UNS
- S24000
- ASTM
- XM-29
- Structure
- Austenitic
- Tensile
- 690 MPa min (100 ksi)
- Yield
- 380 MPa min (55 ksi)
- Elongation
- 40 % minimum
- Density
- 7.775 g/cm³
- Molybdenum
- None not a seawater grade
Chemical composition
The balance that defines the grade: manganese and nitrogen carry the work that nickel does in a 300-series steel, which is why only about 3 % nickel is needed.
| Element | Symbol | Content % | Function |
|---|---|---|---|
| Carbon | C | 0.08 max | Held low to protect grain-boundary corrosion resistance after welding |
| Chromium | Cr | 17.00–19.00 | Passive film; general corrosion and oxidation resistance |
| Manganese | Mn | 11.50–14.50 | Stabilises austenite in place of nickel and raises nitrogen solubility |
| Nickel | Ni | 2.25–3.75 | Deliberately lean, which keeps the grade off the nickel price curve |
| Nitrogen | N | 0.20–0.40 | Main strengthener, interstitial solid solution hardening |
| Silicon | Si | 0.75 max | Residual from deoxidation |
| Phosphorus | P | 0.06 max | Residual, controlled |
| Sulphur | S | 0.03 max | Residual, controlled for hot workability |
| Iron | Fe | Balance | Matrix |
Mill data sheets for Nitronic 33 give silicon as 0.75 % max. Some general supplier listings quote 1.00 % max instead. Where silicon matters to you, name the governing ASTM table on the order and we will certify against that table rather than a generic figure.
Mechanical and physical data
| Property | Metric | Imperial |
|---|---|---|
| Tensile strength | 690 MPa min | 100 ksi min |
| Yield strength, 0.2 % offset | 380 MPa min | 55 ksi min |
| Elongation in 50 mm | 40 % min | 40 % min |
| Hardness, Brinell | 241 HB approx. | 241 HB approx. |
| Hardness, Rockwell B | 100 HRB approx. | 100 HRB approx. |
These are specification minima for the annealed condition. Cold-worked product tests appreciably higher, and individual ASTM classes and section sizes carry their own figures. The acceptance values for your order are those of the specification edition and section size named on the purchase order, not the figures on this page.
| Property | Metric | Imperial |
|---|---|---|
| Density | 7.775 g/cm³ | 0.2808 lb/in³ |
| Thermal expansion, 26–93 °C | 16.07 µm/m·°C | 8.93 µin/in·°F |
| Magnetic response | Low permeability, retained after severe cold work | |
Designations and specifications
One chemistry, several names. Most enquiry confusion on this grade comes from a drawing calling it Nitronic 33 while the purchase order calls it XM-29.
| Specification | Product form | Designation |
|---|---|---|
| ASTM A314 | Stainless billets and bars for forging | S24000 |
| ASTM A276 | Stainless bars and shapes | XM-29 |
| ASTM A479 / A479M | Bars and shapes for boilers and pressure vessels | XM-29 |
| ASTM A240 | Plate, sheet and strip for pressure vessels | XM-29 |
| ASTM A412 | Chromium-manganese-nickel sheet and strip | XM-29 |
| ASTM A312 / A813 / A814 | Seamless and welded pipe | XM-29 |
| ASTM A249 / A269 / A688 | Welded tube | XM-29 |
| ASTM A580 | Stainless wire | XM-29 |
| ASTM A955 / A955M | Deformed reinforcing bar | XM-29 |
No EN, DIN or JIS equivalent is published here, because none is confirmed in the standards we certify to. Other chromium-manganese-nitrogen grades are not interchangeable with S24000 on chemistry. Buy to the UNS number or the ASTM grade.
Forging and heat treatment
S24000 work hardens fast and takes its strength from nitrogen in solution, so the hot-work window and the post-forge anneal matter more than they do on 304.
Hot working
Billet goes in at about 1093 °C (2000 °F) and soaks until the section is through-heated, then comes up to 1177 °C (2150 °F) and equalises before the first blow. Finishing temperature is watched so the piece is never worked cold enough to tear. On heavy upsets and long mandrel work we reheat rather than chase one heat to the end.
Solution annealing
Forgings are solution annealed at 1038 to 1121 °C (1900 to 2050 °F) and quenched rapidly in water or air. That restores full austenite, takes any precipitated phase back into solution and returns ductility and low permeability. Between forming operations we use an intermediate anneal around 1065 °C to shed the stress the alloy builds up as it hardens. The plant runs 14 heat-treatment furnaces including car-bottom units to 8,000 mm long and 15 m deep well furnaces for vertical quenching of shafts.
Hardening, welding, machining
S24000 hardens by cold work only. There is no quench-and-temper route, so a drawing that calls for one on this grade needs correcting before production starts. It welds by the usual processes including GTAW, GMAW and submerged arc. For machining, run slow speeds with positive feed, a sulphurised cutting oil and chip breakers, because the chip comes off tough and stringy. We price machining allowance on that basis rather than quoting 304 cycle times.
What we make in S24000
Everything below is forged from a single piece of steel melted on site. No welding, no casting, no bought-in billet of unknown origin.
| Family | Items |
|---|---|
| Rolled and forged rings | Seamless rolled rings, contoured rings, retaining and containment rings, gear ring blanks, valve seat rings, wear rings |
| Flanges | Weld neck, slip-on, blind, lap joint, socket weld, orifice, long weld neck and special profiles |
| Bars and shafts | Round bar, flat bar, stepped shafts, spindles, eccentric shafts, pins, valve stems |
| Discs and blocks | Solid discs, tube sheets, covers, die and mould blocks, valve bodies and bonnets |
| Hollow sections | Sleeves, bushings, hollow bar, bored cylinders, couplings, nozzles |
| Item | Limit | Set by |
|---|---|---|
| Rolled ring outside diameter | up to 6,000 mm | 6 m radial-axial ring mill |
| Smallest ring | from OD 50 mm | Upset-and-punch route below ring-mill range |
| Shaft turned length | up to 14,000 mm | C61160 lathe, 15 m well furnace for vertical quench |
| Disc and tube sheet diameter | up to 5,000 mm | 5,000 mm vertical turning lathe |
| Bored cylinders | 1,600 mm dia × 10,000 mm | CNC deep-hole drilling machine |
| Single piece weight | up to 30,000 kg | 60 t heat size, 6,300 t open-die press |
| Minimum order | 10 kg | No minimum piece count |
| Lead time | 20 to 60 days | Depends on melt route and test scope |
Supplied as forged and solution annealed, or rough machined, proof machined or finish machined to your drawing.
Where the grade fits
S24000 earns its place where you need strength, non-magnetic behaviour and low-temperature toughness together, in an environment that is not heavily chloride bearing.
| Field | Reason | Forged parts |
|---|---|---|
| Non-magnetic equipment | Low permeability held after heavy cold work | Retaining and containment rings, rotating parts, housings |
| Cryogenic service | Austenite stabilised by manganese and nitrogen | Cold-box valve bodies, flanges, vessel components |
| Valves and pumps | High yield with ductility retained | Bodies, stems, seat rings, tube sheets |
| Rotating machinery | About double the annealed yield of 304 | Fan hubs, shafts, spindles, loaded structural parts |
| Structural and civil | Resists chloride-induced corrosion far better than carbon steel | Anchor and connection forgings, reinforcing bar stock |
Where it does not belong
S24000 carries no molybdenum, so it is not the alloy for seawater, subsea, desalination, flue-gas desulphurisation or strong acid duty, whatever a general stainless page may suggest. Supplier pages that list this grade for subsea piping have copied text from duplex grades. If that is your service, specify one of these instead, all of which we forge:
A182 F51 duplex F53 super duplex F55 super duplex F44 super austenitic 904L Sanicro 28 Incoloy 825 Inconel 625
If the real problem is galling rather than plain strength, Nitronic 60 is usually the better choice in this family. For higher strength with better corrosion resistance, compare Nitronic 50.
Melting, testing and certification
Most forging suppliers in China buy billet. This works starts at the furnace, which matters on a nitrogen-alloyed grade where the melt route controls the property that makes the steel worth buying.
S24000 runs through the 25 t electric arc furnace, is refined in a ladle furnace, then decarburised under vacuum where carbon and nitrogen have to be held inside a tight band. Protective-atmosphere electroslag remelting on the 3 t or 6 t furnace is available where cleanliness or segregation control is critical. Maximum heat size is 60 tonnes. Because melting and forging sit on one site, the certificate traces a finished part back to its melt number instead of stopping at a purchased billet.
| Test | Standard |
|---|---|
| Chemical analysis | Product analysis against the governing ASTM table |
| Tensile and elongation | Per ordered specification and section size |
| Hardness | Brinell or Rockwell as specified |
| Ultrasonic testing | EN 10228-3, SEP 1921 or ASTM A388 to the agreed class |
| Liquid penetrant | ASTM E165 or EN ISO 3452 on request |
| Magnetic permeability | On request, measured after final heat treatment |
| Dimensional report | Against customer drawing with machining allowance recorded |
| Certification | EN 10204 3.1 mill certificate, or 3.2 with third party witness |
Works approvals: CCS, BV, DNV, LR and NK.
Request a quotation
- Drawing in PDF, DWG or STEP, or raw dimensions: OD × ID × height for rings, diameter × length for bars and shafts
- Specification and designation to certify against, for example ASTM A314 S24000 or A479 XM-29
- Quantity and delivery condition: as forged, solution annealed, rough machined or finish machined
- Non-destructive testing class and certificate level, EN 10204 3.1 or 3.2
- Service conditions, meaning temperature, medium and any magnetic permeability limit, so we can confirm S24000 is the right grade before you commit to it
Questions we get asked
Is UNS S24000 the same as XM-29 and Nitronic 33?
Yes. S24000 is the UNS number, XM-29 is the ASTM grade designation used in A240, A276, A312, A479, A955 and others, and Nitronic 33, historically 18-3-Mn, is the trade name. Order by UNS number or ASTM grade and the ambiguity disappears.
Why so little nickel?
By design. Manganese at 11.5 to 14.5 % plus nitrogen at 0.20 to 0.40 % keeps the structure austenitic, so only 2.25 to 3.75 % nickel is needed. The nitrogen also does the strengthening, taking annealed yield to roughly twice that of 304. A lean nickel balance leaves the grade less exposed to nickel price swings than a 300-series equivalent.
Can it be heat treated to higher strength?
No. S24000 hardens by cold work only. The only heat treatment applied is solution annealing at 1038 to 1121 °C with a rapid water or air quench, and that softens and homogenises rather than strengthens. If a drawing specifies quench and temper on this grade, it is an error worth resolving before the steel is melted.
Will it stay non-magnetic after machining?
That is the main reason the grade exists. Mill data describes low magnetic permeability retained even after severe cold working, which is why it is used for containment and retaining rings and other rotating non-magnetic parts. If a maximum permeability figure is contractual, put it on the order so it is measured after final heat treatment rather than assumed.
How does corrosion resistance compare with 304?
At a similar chromium level it offers better resistance to chloride stress corrosion cracking than 304, and in reinforcement use XM-29 resists chloride-induced corrosion far better than carbon steel. It is not a substitute for molybdenum-bearing grades where pitting or crevice attack drives the selection, and it is not an acid-service alloy.
What is the largest S24000 forging you can make?
Rings roll to 6,000 mm outside diameter on the 6 m radial-axial mill, single pieces reach 30 tonnes under the 6,300 t press, shafts turn to 14,000 mm and discs machine to 5,000 mm diameter. The real limit on any given part is the forging reduction ratio you need, so send the drawing and we will confirm in writing whether it can be made in one piece and what ingot size it takes.
Can you supply third-party inspected certificates?
Yes. Standard supply is EN 10204 3.1. EN 10204 3.2 with an independent body witnessing the testing is available, and it should be stated at enquiry stage so the witness points are priced and built into the heat treatment and testing sequence rather than added at the end.
Sources and revision
Composition, mechanical, physical, forging, annealing, welding and machining figures on this page are taken from published mill and supplier data sheets for Nitronic 33 and UNS S24000, together with ASTM grade listings for S24000 and XM-29 in A314, A240, A276, A312, A412, A479, A249, A269, A688, A580, A813, A814 and A955. Plant capability figures are our own. Values here are for selection and reference. The binding figures for any contract are those of the specification edition and section size named on the purchase order.
Page prepared by the technical department, Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province 214423, China. Reviewed 5 October 2026. A plain-text version of this page is available at /Stainless-Steel/UNS-S24000.md.