GRADE UNS S17400 / TYPE 630 FORGING SPEC ASTM A705 GR 630 CONDITIONS A, H900 - H1150-M SOUR SERVICE 33 HRC MAX Markdown version
Jiangyin Jiangnan Metal Melting works and open-die forge, Jiangyin, China Request a quote

Precipitation hardening stainless steel

UNS S17400 Forgings Type 630 seamless rolled rings, flanges, shafts, discs and tube sheets, melted and forged in one works

UNS S17400 is a chromium-nickel-copper precipitation hardening martensitic stainless steel, designated Type 630. It is hardened by a single low-temperature treatment between 900 and 1150 F (482 to 621 C), which both precipitation strengthens and tempers the martensite, reaching 200 ksi (1380 MPa) tensile strength at 44 HRC in the H900 condition. Strength and hardness are held to 600 F (316 C), oxidation resistance extends to about 1100 F (593 C), and creep-rupture strength is useful to 900 F (482 C). Unlike conventional martensitic grades such as Type 410, S17400 is readily weldable.

This works forges the grade to drawing as rings, flanges, shafts, discs, sleeves, bushings and tube sheets, in Condition A or any aged condition from H900 to H1150-M, including the double-aged 33 HRC condition accepted by NACE MR0175 and ISO 15156-3 for sour service.

Grade recordS17400
UNS
S17400
Type
630
Forging
ASTM A705 / ASME SA-705 Gr 630
Aerospace
AMS 5643, AMS 5604, AMS 5825
Bar, plate
ASTM A564, ASTM A693
Sour
NACE MR0175, ISO 15156-3
Melting
EF + LF + VOD, or ESR / VAR remelt
Max piece
30 t, ring OD to 6,000 mm
Min order
10 kg, no minimum count
Lead time
20 to 60 days
01

Designations and specifications

Order against the specification that matches the product form. For forgings that is ASTM A705, not the bar or plate specification, and not a nickel alloy specification.

Specification by product form
ReferenceCovers
ASTM A705 / ASME SA-705, Type 630Age-hardening stainless steel forgings. The primary specification for this page.
AMS 5643Bars, forgings, rings and extrusions. Limited to 8 in. diameter, or 8 in. least distance between parallel sides.
ASTM A564 / ASME SA-564, Type 630Hot-rolled and cold-finished bars, wire and shapes.
ASTM A693 / ASME SA-693, Type 630Sheet, plate and strip.
AMS 5604Sheet, strip and plate.
AMS 5825Welding wire.
NACE MR0175 / ISO 15156-3Sour service for oil and gas production. 33 HRC maximum, double age hardened.
Unified numberUNS S17400.
European numberPublished cross-references differ. Rolled Alloys lists W. Nr. 1.4548 for S17400, while 1.4542 (X5CrNiCuNb16-4) is the number used across much of the European trade. Confirm the exact number when ordering to an EN specification.

ASTM B564 does not apply to this grade. B564 is the specification for nickel and nickel alloy forgings, covering UNS N02200, N04400, N06600, N06603 and N06690 among others. It appears on some S17400 listings in error. For S17400 forgings the correct reference is ASTM A705 or ASME SA-705, Grade 630.

02

Chemical composition

Limits in weight percent, iron balance. Steel for these forgings is melted on site, so the aim chemistry can be set for the part being made rather than accepted as delivered in purchased billet. Ladle analysis is reported on every certificate, and product analysis is available on request.

UNS S17400 composition limits, weight percent
ElementMinimumMaximum
Chromium, Cr15.017.5
Nickel, Ni3.05.0
Copper, Cu3.05.0
Niobium plus tantalum, Cb+Ta5 x C0.45
Carbon, C–0.07
Manganese, Mn–1.00
Silicon, Si–1.00
Molybdenum, Mo–0.50
Phosphorus, P–0.04
Sulphur, S–0.03
Iron, FeBalance

Two points are worth checking against any internal datasheet you hold. Chromium runs to 17.5 percent, not 17.0, so a tighter internal limit will reject conforming heats. Niobium and tantalum are controlled together as one value, with the minimum tied to five times the carbon content rather than fixed.

03

Heat treatment

At the solution treating temperature of 1900 F the structure is austenitic, and it transforms to low-carbon martensite on cooling. That transformation is not complete until the part falls below 90 F (32 C), which is why cooling is taken down properly rather than stopped at room temperature. Ageing then strengthens and simultaneously tempers that martensite, so higher ageing temperatures raise toughness and lower strength. Solution treatment and ageing are carried out here in 14 furnaces, including pit furnaces 15,000 mm deep for vertical treatment of long shafts.

Heat treatment practice by condition
ConditionPracticeResult
A1900 F ± 25 (1040 C), 1/2 hour, air cooled or oil quenched below 90 FSolution treated. Supply and machining condition, not a service condition
H900900 F ± 15 (482 C), 1 hour, air cooledMaximum hardness, low toughness, sensitive to stress-corrosion cracking
H925925 F (496 C), 4 hours, air cooledVery high strength, small gain in toughness
H10251025 F (552 C), 4 hours, air cooledBalanced strength and toughness
H10751075 F (579 C), 4 hours, air cooledHigher toughness, lower strength
H11001100 F (593 C), 4 hours, air cooledHigher toughness again
H11501150 F (621 C), 4 hours, air cooledOveraged, 33 HRC, highest ductility of the single-age conditions
H1150D1150 F, 4 hours, air cool, then 1150 F again, 4 hours, air cool31 HRC. Double aged, improved impact energy. Sour service route
H1150-M1400 F ± 25 (760 C), 2 hours, air cool, then 1150 F ± 15, 4 hours, air cool27 HRC. Highest toughness and best machinability

Condition A is not a service condition. For most applications S17400 should not be used as solution treated, even where the tensile strength in that condition appears to meet the design requirement. Although the material is relatively soft, the structure is untempered martensite with low fracture toughness and ductility, and poor resistance to stress-corrosion cracking. Service performance is assured by using the grade in an aged condition.

Where H900 is specified but impact energy is marginal, ageing for 4 hours instead of 1 hour is the usual remedy. That practice develops typical properties of 196 ksi tensile, 181 ksi yield, 14 percent elongation in 2 in., 52 percent reduction of area, 43 HRC and 20 ft-lb Charpy V-notch, trading roughly 4 ksi of strength for a worthwhile gain in toughness.

04

Mechanical properties

Representative longitudinal tensile properties. These are typical values for selecting a condition, not acceptance criteria. Acceptance is to the minima of the governing specification for the section size and test location, and testing is carried out per order in the delivered condition.

Representative longitudinal properties, room temperature
PropertyH900H925H1025 H1075H1100H1150 H1150DH1150-M
Tensile strength, ksi200190170165150145140125
Tensile strength, MPa138013101170114010351000965860
0.2 % yield, ksi18517516515013512512085
0.2 % yield, MPa1275120511401035930860825585
Elongation in 2 in. or 4D, %1414151617192222
Reduction of area, %5054565858606568
Hardness, Brinell420409352341332311294277
Hardness, HRC4442383635333127
Charpy V-notch, ft-lb15253540455055100
Charpy V-notch, J20344754616875136

Physical properties

Physical properties and temperature dependence
Property70 F212 F392 F572 F
Modulus of elasticity, dynamic, psi x 10629.028.127.026.1
Thermal conductivity, Btu ft / ft2 hr F8.69.29.810.4
Coefficient of thermal expansion from 70 F, in/in F x 10-6–7.27.57.8

Density is 0.282 lb/in³ (7.81 g/cm³), the melting range is 2560 to 2625 F (1404 to 1440 C), Poisson's ratio is 0.272 and electrical resistivity is 463 ohm circular mil per foot. The grade is ferromagnetic in all conditions, which matters if the part sits near magnetic sensing equipment, and which also makes magnetic particle inspection available as an option.

05

Corrosion resistance and sour service

S17400 is corrosion resistant across chemical process service and gives oxidation resistance to about 1100 F (593 C), well beyond the 12 percent chromium martensitic grades it often replaces.

As with every precipitation hardening stainless steel, resistance to stress-corrosion cracking falls as strength rises, and H900 is explicitly the condition most sensitive to it. Where chloride stress-corrosion cracking is credible, age to the lowest strength that still satisfies the design minima rather than to the highest available strength.

For oil and gas production, S17400 is listed in NACE MR0175 and ISO 15156-3 at a maximum hardness of 33 HRC, reached by solution treatment followed by double age hardening, that is the H1150D or H1150-M condition. If the forging is for a wellhead, a Christmas tree, a subsea component or sour valve trim, state that on the enquiry: it fixes the ageing cycle, adds a hardness survey to the test plan, and is not something that can be retrofitted to an already aged part.

06

Forging, machining and welding

Points that affect cost and sequence on a S17400 order.

Machining sequence

Machinability is comparable in character to hardenable grades such as 410, 420 and 430F, but S17400 is considerably stronger and the chips run long. At 44 HRC in H900, turning, drilling and milling are slow with heavy tool wear. The usual sequence is to rough machine in Condition A or in an overaged condition and finish after ageing, allowing for the dimensional change on ageing. Parts machined in H1150-M need a solution treatment before final hardening. Deep-hole drilling to 1,600 mm diameter by 10,000 mm and vertical turning to 5,000 mm diameter are available in-house, so proof machining for volumetric inspection does not go out to a subcontractor.

Welding

This grade is weldable by conventional inert gas methods without preheat, which separates it from conventional martensitic stainless steels. Use matching filler to AMS 5825 followed by post-weld ageing where the weld must respond to heat treatment, or an austenitic filler where it need not. Torch cutting in the annealed condition risks cracking, so saw or water-jet cutting is the safer route on heavy sections.

Working envelope

Size limits for S17400 forgings at this works
ProductLimitSet by
Seamless rolled ringsOD 50 to 6,000 mm6 m radial-axial ring mill, upset and punch route below mill range
Shafts and spindlesto 14,000 mm turned lengthC61160 lathe, 15,000 mm pit furnace for vertical treatment
Discs, tube sheets, blocksto 5,000 mm machined diameter5,000 mm vertical turning lathe
Bored cylinders, hollow shaftsto 1,600 mm dia x 10,000 mmCNC deep-hole drilling machine
Single piece weightto 30,000 kg60 t heat size, 6,300 t open-die press
07

Where this grade is used

Valves

Gate valve components, valve stems, balls, seats, bushings, bodies and bonnets. Sour trim in H1150D or H1150-M.

Pumps and rotating parts

Pump shafts, gears, plungers and sleeves, where strength and corrosion resistance are needed together.

Chemical processing

Process equipment components, nozzles, tube sheets and covers for vessels and heat exchangers.

Wellhead and subsea

Spools, blocks, stems and manifolds for Christmas trees, wellheads, BOPs and risers under API 6A and MR0175.

Rings and flanges

Seamless rolled rings, gear ring blanks, retaining rings, valve seat rings and forged flange blanks.

Fasteners and hardware

Heavy studs, pins and high-strength fittings replacing plated carbon steel where corrosion is a factor.

08

Testing and documents

Because the steel is melted on site, the certificate traces a finished forging back to its melt number rather than stopping at a purchased billet.

Standard scope covers ladle analysis, tensile testing and hardness in the delivered condition, and ultrasonic examination to EN 10228-3, SEP 1921 or ASTM A388 as specified. Charpy V-notch testing, hardness surveys for MR0175 compliance, positive material identification, magnetic particle and liquid penetrant inspection, grain size, intergranular corrosion testing and dimensional reports are available on request. Certificates are issued to EN 10204 3.1, or 3.2 with third-party inspection. The works holds CCS, BV, DNV, LR and NK approvals.

09

Questions

Is UNS S17400 the same as Type 630?

Yes. UNS S17400 is the unified number and Type 630 is the designation used in ASTM and ASME specifications for the same chromium-nickel-copper precipitation hardening stainless steel. Both refer to the grade described on this page. Full detail on the grade, including international cross-references, is on the 17-4PH grade page.

What should the drawing call out?

For a forging, call out the specification, the grade or type, and the condition, for example ASTM A705 Gr 630 Cond. H1025. Without the condition the order is incomplete, because the same chemistry covers tensile strengths from 125 to 200 ksi depending on ageing. Add the NACE requirement separately if the part is for sour service.

Which condition gives the best balance for a pump shaft?

H1025 and H1075 are the conditions usually chosen where strength and toughness both matter, giving 170 and 165 ksi tensile at 38 and 36 HRC with 35 and 40 ft-lb Charpy. H900 is reserved for cases where hardness and strength govern and impact loading is low. The correct choice depends on the design stresses and the environment, so the figures here are for narrowing the options rather than for selecting one.

Can S17400 be supplied remelted?

Yes. Carbon, alloy and stainless grades run through the electric arc furnace, ladle furnace and vacuum oxygen decarburisation. Where a specification calls for remelted material, protective-atmosphere electroslag remelting and vacuum arc remelting are on site, so double-melt requirements do not need a subcontractor.

What is the minimum order?

10 kg, with no minimum piece count, and lead time normally runs 20 to 60 days depending on section size, heat treatment and machining scope.

Pricing a S17400 forging

Send the drawing or the basic dimensions with the specification, the condition, the quantity and any sour service or third-party inspection requirement. Quotations come back with forging weight, the proposed heat treatment route and the test plan.

Email sales@steelforgepieces.com
Telephone 0086-189-2135-9659
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China

Contact page

Published by Jiangyin Jiangnan Metal Co., Ltd., melting works and open-die forge, Jiangyin, Jiangsu, China. Last reviewed 4 October 2026. Composition, heat treatment practice and representative properties compiled from published mill data for UNS S17400 and Type 630, together with ASTM A705, ASTM A564, ASTM A693, AMS 5643 and NACE MR0175 / ISO 15156-3. Values are typical and are given for selecting a condition. They are not acceptance criteria and do not replace the governing specification or project engineering. An independent producer of UNS S17400 forgings, not affiliated with the owner of any trademark referenced in the standards cited.