GRADE SUS 317 / AISI 317 / UNS S31700 / EN 1.4449 WORKS No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu, China +86 189 2135 9659   sales@steelforgepieces.com
Jiangyin Jiangnan Metal Melting works · Open-die forge · Ring mill · Since 1997 Request a quote

Home / Stainless steel / SUS 317

Material datasheet · Austenitic stainless steel

SUS 317 Forgings AISI 317 · UNS S31700 · EN 1.4449 · ASTM A182 F317

SUS 317 is a molybdenum-bearing austenitic stainless steel, in effect a higher chromium, nickel and molybdenum version of 316. It contains 18.0 to 20.0 percent chromium, 11.0 to 15.0 percent nickel and 3.0 to 4.0 percent molybdenum, with carbon held to 0.08 percent maximum. The extra molybdenum is what the grade is bought for: it raises strength and improves resistance to pitting and crevice attack in chloride-bearing, moderately oxidising and reducing media, so 317 goes in where 316 is marginal.

This works forges the grade to drawing rather than to a stock list. Steel is melted on site, forged or ring-rolled, solution annealed, machined and tested without leaving the plant, so the certificate traces back to a melt number instead of stopping at a purchased billet.

Grade summaryS31700
Type
Austenitic
UNS
S31700
Forging spec
ASTM A182 / SA182 F317
EN number
1.4449
Key element
Molybdenum 3.0–4.0 %
Anneal
1010–1121 °C, then cool
Hot work
1149–1260 °C
Max ring OD
6,000 mm
Max piece
30 t
Minimum order
10 kg, no piece minimum
Lead time
20 to 60 days
Certificate
EN 10204 3.1, or 3.2 witnessed
01

Chemical composition

The limits below are the ASTM A182 Grade F317 forging requirement. Chemistry is read at the furnace on a mobile optical emission spectrometer and confirmed on the finished part with a handheld analyser, so the analysis printed on the certificate is this plant's own rather than a supplier's.

SUS 317 / UNS S31700 composition, weight percent
ElementSymbolSpecifiedNominal
CarbonC0.08 max–
ChromiumCr18.0–20.019
NickelNi11.0–15.013
MolybdenumMo3.0–4.03.5
ManganeseMn2.00 max–
SiliconSi1.00 max–
PhosphorusP0.045 max–
SulphurS0.030 max–
IronFeBalance61

Low-carbon 317L (UNS S31703) is available where post-weld sensitisation is a concern. State which of the two you need on the enquiry.

02

Mechanical properties

Two sets of numbers matter here and they are not interchangeable. The first is what a forging has to achieve on test to be certified. The second is what annealed material of this grade typically measures. Buyers write the first into the purchase order; the second is useful for early design estimates.

Specified minimums, ASTM A182 F317

Required minimum values for forgings
PropertyMetricImperial
Tensile strength, min515 MPa75 ksi
Yield strength 0.2 % offset, min205 MPa30 ksi
Elongation in 50 mm or 4D, min30 %30 %
Reduction of area, min50 %50 %

Typical annealed values

Published typical properties, grade 317 annealed
PropertyValue
Tensile strength620 MPa
Yield strength275 MPa
Elastic modulus193 GPa
Poisson's ratio0.27 to 0.30
Elongation at break, 50 mm45 %
Hardness, Rockwell B85

Typical values are not acceptance criteria. Results shift with section size, forging reduction and where the test piece is cut. Tensile testing here runs on 600 kN and 300 kN machines to ASTM A370 and ISO 6892.

03

Physical properties

Grade 317 physical data
PropertyMetricImperial
Density8.0 g/cm³0.289 lb/in³
Melting point1370 °C2550 °F
04

Forging and heat treatment route

SUS 317 takes all the common hot-working methods. Stock is heated to 1149 to 1260 °C and the pass schedule is planned so the workpiece is off the press before it drops below 927 °C. Working colder risks cracking and leaves residual strain that costs corrosion resistance later.

After forging or ring rolling, parts are solution annealed at 1010 to 1121 °C and cooled. That step returns carbides to solution and restores the corrosion performance the grade was specified for, so it is not optional on anything going into chloride service. The grade does not respond to hardening heat treatment. Strength above the annealed condition can only come from cold work, and cold-worked parts should be annealed afterwards to relieve internal stress.

Machining is tougher going than on 304. Chip breakers help, and a constant feed at moderate speed works better than running slow. Discs and tube sheets are supplied proof-machined so the ultrasonic probe sits on a clean surface.

Melting

Electric arc furnace with ladle refining and vacuum oxygen decarburisation, which is the route that holds carbon down in a grade capped at 0.08 percent. Heats to 60 t.

Forging

Hydraulic presses at 6,300 t, 4,000 t and 2,000 t, five hammers from 750 kg to 5 t, and radial-axial ring mills at 1 m, 3 m and 6 m.

Heat treatment

14 furnaces, including car-bottom chambers to 8,000 by 2,000 by 2,000 mm and two 15 m well-type furnaces for quenching long shafts vertically.

Machining

Vertical lathes to 5,000 mm swing, horizontal lathes to 14 m between centres, CNC deep-hole drilling to 1,600 by 10,000 mm.

05

Product forms in SUS 317

Everything is made to drawing or to a stated rough size. There is no catalogue of fixed dimensions and no minimum piece count: the floor is 10 kg by weight.

SUS 317 forged product forms and size limits
FormCoversSize limit
Seamless rolled ringsRectangular and contoured section, gear ring blanks, slewing rings, bearing racesOD 50 to 6,000 mm
Forged ringsUpset and punched rings, retaining rings, valve seat ringsOutside the ring-mill envelope
FlangesWeld neck, blind, slip-on, socket weld, lap joint, orifice, long weld neckTo ASME B16.5 and B16.47
Bars and blocksRound, flat and square bar, blanks for machined valve bodiesPress and lathe limits
Discs and tube sheetsSolid discs, tube sheets, covers, hubs, proof-machined for ultrasonic testingTo 5,000 mm machined diameter
Shafts and spindlesStepped shafts, eccentric shafts, spindles, rolls, pinionsTo 14,000 mm turned length
Cylinders and sleevesBored hollows, sleeves, bushings, nozzles, heavy-wall pipe sectionsTo 1,600 by 10,000 mm bored
Valve partsBodies, bonnets, stems, seat rings, blocks, manifoldsTo drawing

Heaviest single piece in any of these forms is 30 t, set by the 60 t heat size and the 6,300 t press.

06

Where the grade is used

317 is a pulp and paper, textile and chemical process grade before anything else. Common end uses for forged components in it fall into four groups.

Pulp and paper

Digesters, liquor tanks, paper machine components, and the flanges, tube sheets and valve parts that go with them. This is the classic home for the extra molybdenum.

Chemical process

Absorber towers, heat exchangers, pressure vessels, slurry tanks, stack liners and scrubber internals, where service is moderately oxidising or reducing and chloride is present.

Refining and recovery

Catalytic recovery systems, recuperators, and the forged pipe sections, tube sheets and flanges that go into them.

Valves and rotating parts

Bodies, stems and seat rings for ball, gate, globe, check and plug valves, plus shafts, gear blanks and spindles in power transmission duty.

07

Designations and product standards

SUS 317 is the Japanese-style designation for this grade. Orders are normally placed against the UNS number or the ASTM product specification, and that is what the certificate will reference.

SUS 317 cross-reference
System or product formDesignation
UNSS31700
AISI / SAE317, SAE 30317
EN / DIN1.4449
Forgings and piping componentsASTM A182 / ASME SA182 F317
Plate and sheetASTM A240 / ASME SA240
Bar and shapesASTM A276, A473, A479
Pipe and tubeASTM A312, A213, A249, A269
FittingsASTM A403 / ASME SA403
Low-carbon variant317L, UNS S31703
08

Testing and certification

The works runs its own laboratory. A SUS 317 forging is released against a documented route: melt analysis, mechanical testing on a representative test piece, non-destructive examination, dimensional inspection, then certification.

Standard scope for a SUS 317 order
StageMethodReference
Chemical analysisOptical emission spectrometry, infrared carbon and sulphurASTM E415, ASTM E1019
Alloy verificationHandheld analyser, positive material identificationPMI
Tensile600 kN and 300 kN universal testing machinesASTM A370, ISO 6892
ImpactPendulum machine with low-temperature bathASTM A370
UltrasonicDigital flaw detection on proof-machined surfacesASTM A388, EN 10228-3
Magnetic particleWhere applicable to the componentASTM E709
Grain sizeMetallographyASTM E112
CertificateMill test certificate, or witnessed by a third-party inspection bodyEN 10204 3.1 / 3.2

Intergranular corrosion testing to ASTM A262 or G28 and pitting resistance to ASTM G48 are placed with an accredited outside laboratory and reported alongside the mill certificate. Ask at enquiry stage so they are scheduled before shipment rather than added afterwards.

09

Questions about this grade

What is SUS 317 stainless steel?

SUS 317 is the Japanese-style designation for the 317 molybdenum-bearing austenitic stainless steel, covered elsewhere as AISI 317, UNS S31700 and EN 1.4449. It runs 18.0 to 20.0 percent chromium, 11.0 to 15.0 percent nickel and 3.0 to 4.0 percent molybdenum with carbon at 0.08 percent maximum, which makes it a higher chromium, nickel and molybdenum version of 316 with more strength and better corrosion resistance.

How does SUS 317 differ from 316?

Molybdenum. SUS 317 carries 3.0 to 4.0 percent against roughly 2 to 3 percent in 316, with chromium and nickel also lifted. That extra molybdenum buys resistance to pitting and crevice attack in chloride-bearing and moderately reducing service, which is the reason the grade shows up in pulp and paper and scrubber duty where 316 is borderline. It costs more, so it is worth confirming the service genuinely needs it.

What does a SUS 317 forging have to test at?

Under ASTM A182 Grade F317 the minimums are 515 MPa tensile strength, 205 MPa yield strength, 30 percent elongation in 50 mm or 4D, and 50 percent reduction of area. Published typical values for annealed material sit above that at roughly 620 MPa tensile, 275 MPa yield, 45 percent elongation and Rockwell B 85, with an elastic modulus of 193 GPa. Write the specification minimums into the order, not the typical figures.

What are the forging and annealing temperatures?

Hot work between 1149 and 1260 °C, and stop before the piece falls below 927 °C. Solution anneal afterwards at 1010 to 1121 °C followed by cooling. The grade cannot be hardened by heat treatment, only by cold work, and cold-worked parts should be annealed to relieve stress.

How large a SUS 317 part can this works produce?

Seamless rings roll up to 6,000 mm outside diameter on the 6 m radial-axial mill, with 3 m and 1 m mills for smaller sizes. The heaviest single forging is 30 tonnes, worked on 6,300 t, 4,000 t and 2,000 t presses. Downstream equipment sets the practical limits: furnaces take work to 8,000 by 2,000 by 2,000 mm, two 15 m well furnaces allow long shafts to be quenched vertically, vertical lathes machine to 5,000 mm swing and horizontal lathes to 14 m between centres.

Is there a minimum order, and how long does it take?

Minimum order is 10 kg with no minimum piece count, so a single part is quotable. Lead time runs 20 to 60 days from order confirmation. SUS 317 sits at the lower end of that band because it is melted through the electric arc furnace and refined without a remelting step. Witnessed inspection or outside corrosion testing needs scheduling, so flag either at enquiry stage and it will be built into the quoted date.

Can 317L be supplied instead?

Yes. 317L, UNS S31703, is the low-carbon variant and is the usual choice where components will be welded and then exposed to aggressive service, since the lower carbon limits carbide precipitation at the weld. State which of the two you need on the enquiry, because the two are not interchangeable on a certificate.

10

Request a quotation

Quotations come from a drawing or a written specification. Sending the six items below in the first email removes a round trip and usually gets a price back within two working days.

What to include
#ItemExample
1Grade or specificationASTM A182 F317 / UNS S31700
2Dimensions, or a drawing in PDF, DWG, DXF or STEPOD 1200 x ID 900 x H 260 mm
3Quantity and expected repeat volume8 pcs, about 3 per year
4Delivery conditionProof-machined
5Heat treatment and testingSolution annealed, UT to ASTM A388
6Certification and destination portEN 10204 3.2 witnessed, Rotterdam