GRADE AISI 631 / 17-7 PH  ·  UNS S17700  ·  EN 1.4568 JIANGYIN, JIANGSU, CHINA  ·  +86 189 2135 9659  ·  SALES@STEELFORGEPIECES.COM
Jiangnan Metal Melting works  /  Open-die forge  /  Ring mill Request quote

Home / Stainless Steel / AISI 631

AISI 631 Forgings 17-7 PH precipitation-hardening stainless steel, UNS S17700, forged to ASTM A705 Grade 631 and AMS 5644

A chromium-nickel-aluminium stainless steel that is soft and austenitic as annealed, then transformed and aged to very high strength with little distortion. We melt it in our own furnaces and forge it into rings, flanges, shafts, discs and bars without the part leaving the works.

Grade data sheetS17700
Grade
AISI 631 / 17-7 PH
Equivalents
UNS S17700 · EN 1.4568 · X7CrNiAl17-7 · JIS SUS 631
Forging specs
ASTM A705 Gr 631 · ASME SA705 · AMS 5644 · ASTM A564 Type 631
Conditions
A · A1750 · T · R100 · TH 1050 · RH 950
Melting
EF + LF + VOD, or ESR / VAR remelt for fatigue-critical work
Max ring OD
6,000 mm on the radial-axial mill
Max single piece
30,000 kg
Certification
EN 10204 3.1, or 3.2 with third-party witnessing
Lead time
20 to 60 days · minimum order 10 kg
01

The grade in practice

Type 631 is the AISI designation for the alloy sold as 17-7 PH. The numbers are the nominal chromium and nickel contents. Hardening comes from an aluminium addition rather than the copper used in 17-4 PH, and that single difference changes how the material is supplied, machined and heat treated.

As delivered in Condition A the structure is austenitic, soft and formable. Strength is developed afterwards, by conditioning the austenite, cooling to convert it to martensite, then ageing at low temperature. Because the ageing step runs at 510 to 566 °C rather than a quench-and-temper cycle, dimensional movement stays small and predictable. That is the reason the grade survives in applications where close tolerances have to come through heat treatment intact.

The alloy holds useful spring properties up to roughly 316 °C and is long established in aircraft structural parts, instrument and control components, diaphragms, retaining rings and flat springs.

Before you specify 631 for a forging

For machined or forged parts that are not used alongside 17-7 PH sheet or plate, the published guidance from the alloy's originating producer points elsewhere. 17-4 PH and 15-5 PH reach similar strength with higher impact strength and comparable corrosion resistance. PH 13-8 Mo goes higher on both tensile and impact strength with better corrosion resistance, and is the grade named for components loaded in the transverse direction.

We forge all of them, along with Nitronic 50, A-286 and the full nickel alloy range. Tell us the duty and we will quote the grade that fits rather than the one on the enquiry.

02

Specifications and equivalents

Half the enquiries we see for this grade arrive against a flat-product specification or a nickel alloy standard. The table separates what applies to a forging from what does not.

Specification by product form
SpecificationProduct formApplies to forgings
ASTM A705 / SA705 Gr 631Age-hardening stainless steel forgingsYes, primary
AMS 5644Bars and forgingsYes, primary for aerospace
ASTM A564 / SA564 Type 631Bars and shapesYes, for forged and rolled bar
ASTM A579Superstrength alloy steel forgingsYes, where invoked
ASTM A693 / SA693Plate, sheet and stripNo
AMS 5528 / AMS 5529Sheet, strip and plateNo
ASTM A313 / AMS 5678Spring wire and wireNo
AMS 5568Welded tubingNo
AMS 5824Welding wireNo, filler only
ASTM B564 is not a 631 specification

B564 covers nickel and nickel-copper alloy forgings for general corrosion service and pressure vessel use. It has no stainless steel grades in it. Where a B564 callout appears against 631 it is almost always carried over from a nickel alloy line on the same drawing, and we raise it at quotation rather than issue a certificate to the wrong standard. The forging specifications are A705, SA705, AMS 5644 and A564 Type 631.

Composition limits, weight per cent, balance iron
StandardCMnSiPSCrNiAl
UNS S17700, AMS0.09 max1.00 max1.00 max0.040 max0.030 max16.00-18.006.50-7.750.75-1.50
EN 1.45680.09 max1.00 max0.70 max0.040 max0.015 max16.0-18.06.5-8.30.70-1.50
JIS SUS 6310.09 max1.00 max1.00 max0.040 max0.030 max16.00-18.006.50-7.750.75-1.50

The windows are not interchangeable. EN caps sulphur at 0.015 and silicon at 0.70, and runs nickel to 8.3. Some ASTM flat-product tables tighten phosphorus and sulphur to 0.025 and narrow chromium to 16.00-17.25. Name the governing standard on the order and the heat is melted to that window.

Melting route

Standard route is electric arc furnace, ladle refining, then vacuum oxygen decarburisation, with a maximum heat size of 60 tonnes. Where the part sees cyclic stress, remelted material is the better buy: electroslag or vacuum arc remelting gives a further increase in fatigue resistance, and both furnaces are on site, so a double-melt requirement does not go out to subcontract.

03

Heat treatment

631 does not use the H 900 to H 1150 codes that engineers know from 17-4 PH and 15-5 PH. Reaching full strength from Condition A takes three separate operations, and the second one is the step most often missed.

Standard treatments
ConditionAustenite conditioningTransformationPrecipitation hardening
ASolution anneal 1038 ± 14 °C, 30 min minimum. Hot-worked and forged material: 1038 ± 6 °C, 30 min minimum, water quench. Result is austenitic and formable.
TH 1050760 ± 14 °C, hold 90 minCool within 1 h to 16 °C, hold 30 min minimum, giving Condition T566 ± 6 °C, hold 90 min, air cool
RH 950954 ± 9 °C, hold 10 min, air cool, giving Condition A1750Cool within 1 h to minus 73 ± 6 °C, hold 8 h, giving Condition R100510 ± 6 °C, hold 1 h, air cool
C, CH 900Flat and wire product only. Martensite is produced by cold reduction at the mill, then aged at 482 ± 6 °C for 1 h. Not a forging condition.
Two things that go wrong

RH 950 cannot be produced without genuine sub-zero capability and an eight-hour hold at minus 73 °C. Any supplier quoting RH 950 should be able to show the time at temperature on the chart. Ours is recorded and shipped with the parts.

Ageing is a peak-strength reaction. Going hotter or longer than the specified cycle takes the material past peak and deliberately lowers strength, which is useful when a drawing calls for an intermediate level but means an over-aged part cannot simply be aged again. Recovery needs a full re-solution treatment from 1038 °C.

Our heat treatment capacity is 14 furnaces, including eight car-bottom furnaces up to 8,000 × 2,000 × 2,000 mm and two well-type furnaces 15,000 mm deep by 1,500 mm diameter, which is what allows long shafts to be solution treated and quenched hanging vertically rather than laid down.

04

Mechanical and physical properties

The figures below are for bar, rod and forgings. Sheet and strip minima from AMS 5528 and AMS 5529 are commonly reproduced on forging pages and they do not apply to a forged ring or shaft.

Minima for bar, rod and forgings, sections to 76.2 mm inclusive
ConditionTensile MPa (ksi)0.2 % yield MPa (ksi)Elongation % in 4DReduction of area %Hardness
A, as received1034 (150) maxnot specifiednot specifiednot specified229 HB max, B98 max
TH 10501172 (170) min965 (140) min6 min25 min363 HB min, C38 min
RH 9501276 (185) min1034 (150) min6 min10 min387 HB min, C41 min

Note the reduction of area: RH 950 is the stronger condition but is allowed only 10 per cent against 25 per cent for TH 1050. Typical rather than minimum room-temperature values run near 1207 MPa tensile and 1069 MPa yield at 402 HB for TH 1050, and near 1379 MPa tensile and 1207 MPa yield at 430 HB for RH 950. Design to the minima.

Typical physical properties by condition
PropertyCondition ATH 1050RH 950
Density, g/cm³7.817.657.65
Modulus of elasticity, GPa200200200
Modulus of rigidity, GPa757575
Mean expansion 21-93 °C, µm/m·K15.310.010.3
Electrical resistivity, µΩ·cm808283
Magnetic responseWeakly ferromagneticStrongly ferromagneticStrongly ferromagnetic

Thermal expansion drops by roughly a third between Condition A and the hardened conditions, and magnetic permeability changes substantially. Both matter if the part has to match a mating component's growth or sits close to a sensor.

05

Forging, machining and welding

Forging

Practice follows Type 302 closely. Forging temperature should not exceed 1232 °C, and depending on section size and shape the material can be worked at 1177 °C or below, which cuts scale loss. There is no intermediate range in which the steel must not be worked, and charging into a hot or a cold furnace is both acceptable. After forging the part may be air cooled or quenched in oil or water, then solution treated at 1038 °C and water quenched to return it to Condition A.

On this site that work runs on a 6,300 t press backed by 4,000 t and 2,000 t presses, five hammers from 750 kg to 5 t, and three radial-axial ring mills covering 1,000, 3,000 and 6,000 mm outside diameter. Rings below the mill range are produced by the upset-and-punch route from 50 mm outside diameter upward.

Machining

Condition A machines like Type 302 and work-hardens fast, so keep the feed positive and do not let the tool dwell. Once transformed and aged, the material cuts like any steel of the same hardness, which means normal practice for the 275 to 400 BHN range. Where the drawing allows it, the sensible sequence is rough machining in Condition A, heat treatment, then finishing. It is cheaper and it holds tolerance better than cutting fully hardened TH or RH stock.

Welding

631 welds by conventional inert-gas methods and does not need the preheat or post-weld anneal that the standard hardenable stainless steels require. Shielding is not optional, though. The hardening reaction depends on aluminium, which is reactive, and losing it to the atmosphere costs strength that no later heat treatment will recover. As-welded metal is largely austenitic with properties close to Condition A, so a high-strength joint needs the whole post-weld sequence of solution anneal, austenite conditioning, transformation and ageing.

06

Corrosion resistance and its limits

631 is a strength grade with moderate corrosion resistance. Specified on that basis it performs well. Specified as a corrosion-resistant alloy it disappoints, and in one environment it fails outright.

In TH 1050 and RH 950 the resistance is generally better than the standard hardenable chromium stainless steels such as Types 410, 420 and 431, and not quite as good as chromium-nickel Type 304. Condition CH 900 approaches 304 in most environments. In marine atmosphere exposure the ranking runs Type 301 first, then CH 900, then TH 1050, then RH 950, so performance slips slightly as strength rises. Superficial rust can appear in aggressive atmospheres; after the first six months the amount changes little over one to two years.

Hydrogen sulphide service

Like all martensitic stainless steels, 631 may crack when exposed under stress to environments containing hydrogen sulphide. In published testing, Condition CH 900 springs cracked readily in synthetic sour well solution made up of 5 per cent sodium chloride and 0.5 per cent acetic acid saturated with H₂S. The alternatives named in that same guidance are cold-drawn Type 304, Nitronic 50 and the age-hardenable A-286.

We will not quote 631 for H₂S-bearing wellhead or downhole duty without a written NACE MR0175 and ISO 15156 review. For that work ask about our nickel alloy forgings, or about Nitronic 50 and A-286, all of which we melt and forge here.

Precipitation-hardening stainless steels can also fail by stress-corrosion cracking under particular combinations of hardness, sustained tensile stress and environment. Where that risk exists, the lower-strength condition aged at the higher temperature is the safer specification.

07

What we make in AISI 631

Seamless rolled rings

Ring-rolled from a punched preform on the radial-axial mills, rectangular or contoured section, from 50 mm up to 6,000 mm outside diameter.

Forged rings

Upset and punched rings for sections outside the mill envelope, retaining rings and valve seat rings.

Shafts and spindles

Stepped, gear, pinion and eccentric shafts, turned to 14,000 mm length, vertically quenched in the 15 m well furnaces.

Flanges

Weld neck, blind, slip-on, socket weld, lap joint and orifice patterns, and custom profiles to drawing.

Discs, blanks and tube sheets

Upset discs, gear and coupling blanks, tube sheets and covers, machined to 5,000 mm diameter and supplied proof-machined for volumetric inspection.

Sleeves, bushings and hollows

Mandrel-forged or bored hollows to 1,600 mm diameter by 10,000 mm on the CNC deep-hole drilling machine.

Bars and blocks

Forged round, square and flat bar as feedstock for machined valve and instrument parts.

Valve parts

Stems, seat rings, bodies, bonnets, blocks and spools for clean-media service.

Where it is used

631 is chosen for strength-to-weight, fatigue life and dimensional stability rather than for aggressive corrosion duty. That puts it in aerospace structural and control components, flat and helical springs, spring washers and diaphragms working up to about 316 °C, pump and compressor shafts and sleeves, valve stems and internals in clean media, instrument and actuator parts, fasteners and retaining components, and general machine elements under cyclic load. For hot gas, high-chloride, strongly acidic or sour service, a nickel alloy or an austenitic grade is the right answer and we would rather quote you that.

08

Inspection and documents

Because the steel is melted here, the certificate traces a part back to its melt number rather than stopping at a purchased billet.

Chemical analysis is reported per heat. Mechanical testing covers tensile, hardness and, where specified, impact, on test blanks heat treated in the same furnace load as the production parts, which is the only arrangement under which the certificate describes what you actually receive. Ultrasonic examination is carried out to EN 10228-3, SEP 1921 or ASTM A388 as specified, and dye penetrant to ASTM E165 on finished surfaces. Dimensional reports and heat-treatment charts ship with the parts, certified to EN 10204 3.1, or 3.2 where third-party witnessing is required. The works holds CCS, BV, DNV, LR and NK approvals.

One scheduling point worth raising at enquiry stage: in Condition A the structure is austenitic and ultrasonically noisier than it is after transformation. Where acceptance to EN 10228-3 is required, the examination should be scheduled after transformation, and we need the acceptance class in advance so the correct test stock is left on the forging.

09

Questions we are asked

Which specification applies to AISI 631 forgings?
ASTM A705 Grade 631 and ASME SA705 for age-hardening stainless steel forgings, AMS 5644 for bars and forgings in aerospace work, and ASTM A564 or SA564 Type 631 for bars and shapes. ASTM B564 does not cover this grade, because it is a nickel and nickel-copper alloy forging specification.
What delivery conditions can you supply?
Condition A, A1750, the intermediate conditions T and R100, and the hardened conditions TH 1050 and RH 950. Conditions C and CH 900 need cold reduction and so exist only in sheet, strip and wire. The H 900 to H 1150 codes belong to 17-4 PH and 15-5 PH.
What is the difference between 630 and 631?
Type 630, or 17-4 PH, hardens through copper, arrives martensitic and is aged in the H conditions. Type 631, or 17-7 PH, hardens through aluminium, arrives austenitic and formable, and has to be austenite conditioned and transformed before ageing. 631 earns its place in springs, diaphragms and thin sections where distortion must stay small. In heavy forgings, 17-4 PH, 15-5 PH and PH 13-8 Mo generally give higher impact strength.
Can 631 go into sour service?
Not without qualification against NACE MR0175 and ISO 15156. It can crack when held under stress in hydrogen sulphide, and Condition CH 900 material cracked readily in laboratory synthetic sour well solution. Cold-drawn austenitic stainless, Nitronic 50 and A-286 are the published alternatives.
What are the equivalent grades?
AISI and ASTM Type 631 equals 17-7 PH, UNS S17700, EN 1.4568 or X7CrNiAl17-7, and JIS SUS 631. Silicon, sulphur and nickel limits differ between the standards, so state which one governs.
How hard is it to machine once aged?
TH 1050 and RH 950 run 363 to 387 HB minimum, which is 38 to 41 HRC. Follow normal practice for 275 to 400 BHN steel: rigid setup, carbide tooling, positive feed, plenty of coolant. Roughing in Condition A first is almost always cheaper.
Is it magnetic?
Condition A is austenitic and only weakly ferromagnetic. After transformation to martensite in T, R100, TH 1050 and RH 950 it is strongly ferromagnetic. If the assembly is magnetically sensitive, specify the delivery condition on the order.
What is the smallest order you take?
10 kg, with no minimum piece count. Lead time on 631 runs 20 to 60 days depending on size, melting route and the heat-treatment sequence.
10

Quote an AISI 631 forging

Send a drawing, or just the dimensions, grade, delivery condition and quantity. You get back a price, the process route we intend to use, the test plan and a lead time.

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
+86 189 2135 9659