Jiangyin Jiangnan Metal Co., Ltd.Open-Die Forging Factory
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu, China
Tel 0086-189-2135-9659  |  sales@steelforgepieces.com

Home › Stainless Steel › AISI 348

AISI 348 (UNS S34800) Forgings

Columbium-stabilized austenitic stainless steel · ASTM A182 Grade F348 · SAE 30348

AISI 348 is an 18Cr-8Ni austenitic stainless steel stabilized with columbium and tantalum, and it carries two limits that ordinary stabilized grades do not: cobalt 0.20 % max and tantalum 0.10 % max. Those ceilings are the reason the grade is written into nuclear work. We forge it to ASTM A182 Grade F348 as rolled rings, flanges, shafts, discs and bars.

The stabilizing addition ties up carbon as niobium carbide instead of chromium carbide, so chromium stays in solution and the steel resists intergranular attack after exposure in the sensitizing range. AZoM groups 348 with 321 on that basis. What separates 348 from the rest of the stabilized family is the composition ceiling on cobalt and tantalum, both of which become activated under neutron flux. Order the grade when the specification calls for it by name; if your print says 347 and nothing about cobalt, 347 is cheaper and easier to source.

Forms We Supply

Seamless rolled rings

Bearing races, retaining rings, slewing ring blanks, pump wear rings. Rolled from an upset and pierced blank so the grain follows the circumference.

Flanges and fittings

Weld neck, slip-on, blind, long weld neck, orifice and spectacle blinds to ASME B16.5 and B16.47 dimensions, in A182 F348.

Shafts, stepped shafts, spindles

Open-die drawn out with intermediate upsetting to keep the reduction ratio honest through the full length.

Discs, blanks and tube sheets

Upset discs and pierced blanks for valve bodies, closures, covers and heat exchanger tube sheets.

Sleeves, bushings and hollows

Forged and bored hollow sections, saving machining time against solid bar on thin-wall parts.

Forged bar and billet

Round, square and flat forged bar for re-machining. Forged bar, not rolled bar, where the print demands forged product.

Chemical Composition

Table 1. ASTM A182 / A182M Grade F348, UNS S34800. Percent by mass, single values are maxima.
ElementA182 F348 limit, %Typical for grade 348, %
Carbon0.08 max0.08
Manganese2.00 max2.0
Phosphorus0.045 max0.045
Sulfur0.030 max0.030
Silicon1.00 max1.0
Chromium17.00 - 20.0019
Nickel9.00 - 13.0011
Columbium + tantalumsee note below0.8
Cobalt0.20 max0.2
Tantalum0.10 max0.1
Ironbalance66
On the columbium minimum. The ASTM A182 footnote requiring columbium of not less than eight times the carbon content, and not more than 1.10 %, is written against Grades F347H and F348H. It is not the rule for plain F348. If your application needs that ratio guaranteed, order F348H and state it on the purchase order.

Mechanical Properties

Two sets of numbers matter here and they are not interchangeable. The A182 column is what we certify and what the material is accepted against. The annealed column is what the metal usually tests at.

Table 2. Specified minima for A182 F348 against typical annealed values for grade 348.
PropertyA182 F348, minimumTypical, annealed
Tensile strength515 MPa [75 ksi]655 MPa [95 000 psi]
Yield strength, 0.2 % offset205 MPa [30 ksi]275 MPa [39 900 psi]
Elongation, 50 mm [2 in] or 4D30 %45 %
Reduction of area50 %not stated
Hardness, Rockwell Bnot specified in A18285 HRB
Hardness, Brinellnot specified in A182147 HB, converted from HRB
Hardness, Vickersnot specified in A182169 HV, converted from HRB
Izod impactnot specified in A182120 - 160 J [88.5 - 118 ft-lb]
Charpy impactnot specified in A182160 J [118 ft-lb]
Modulus of elasticity-190 - 210 GPa
Shear modulus-77.0 GPa
Poisson's ratio-0.27 - 0.30

Physical and Thermal Data

Table 3. Grade 348, room temperature unless noted.
PropertyMetricImperial
Density8.0 g/cm³0.289 lb/in³
Melting point1427 °C2600 °F
Coefficient of thermal expansion, 0 - 100 °C17.3 µm/m·°C9.61 µin/in·°F
Thermal conductivity at 100 °C16.3 W/m·K113 BTU·in/hr·ft²·°F

Hot Working and Heat Treatment

Forging range

Hot work between 1149 and 1232 °C (2100 to 2250 °F). Do not continue forging below 927 °C (1700 °F); reheat instead. After hot work the part is water quenched or fully annealed to put the corrosion resistance back.

Annealing

Anneal at 1010 to 1093 °C (1850 to 2000 °F), then quench in water. Forgings ordered to A182 Grade F348 are supplied solution treated and quenched, and the certificate states the temperature and the quench medium used.

Hardening

Grade 348 does not respond to hardening heat treatment. There is no quench-and-temper cycle and no aging cycle for this steel. Higher strength is available only through cold reduction, which costs ductility. Anyone quoting you a hardened or aged condition in 348 has the wrong grade.

Fabrication

Machining

Slightly tougher than 304. Use constant positive feed and slow speed; dwelling work-hardens the cut surface and the next pass pays for it. Rigid setup, sharp tooling, generous coolant.

Welding

Joined by fusion and resistance welding. Oxyacetylene welding is not preferred for this alloy. Filler metal AWS E348 or ER348 where filler is required.

Cold working

Ductile and tough. Readily blanked, stamped, drawn and spun. Expect springback and work hardening typical of the austenitic family.

Corrosion behaviour

The columbium and tantalum addition raises intergranular corrosion resistance. Grade 348 is not a pitting-resistant alloy; chloride service belongs to a molybdenum-bearing or duplex grade.

Equivalent and Related Designations

Table 4. Designations listed for grade 348.
UNSS34800. The high-carbon version is S34809 (348H).
SAESAE 30348, SAE J405 (30348)
ASTM, forgings and barA182, A276, A314, A336, A479, A580, A632
ASTM, plate, sheet, pipe, tubeA167, A213, A240, A249, A269, A312, A358, A376, A403, A409, A813, A814
ASMESA182, SA213, SA240, SA249, SA312, SA358, SA376, SA403, SA409, SA479
Military and federalMIL-S-23195, MIL-S-23196, QQ-S-766
EuropeanDesignation tables for grade 348 point to DIN 1.4550. Note that 1.4550 is itself X6CrNiNb18-10 / AISI 347 / UNS S34700. No EN material number reproduces the cobalt and tantalum ceilings of S34800, so a 1.4550 certificate is not a substitute when those limits are the point of the order.

Size and Weight Limits

ASTM A182 / A182M limits products made to that specification to a maximum weight of 10 000 lb [4540 kg]. Above that figure the standard itself refers you elsewhere: ASTM A965 / A965M for austenitic steel forgings for high-temperature service, and ASTM A336 / A336M for pressure and high-temperature parts. If your 348 forging will finish heavier than 4540 kg, fix the specification at the enquiry stage. Changing it after the ingot is poured is expensive.

Where the Grade Gets Used

Grade 348 is used in nuclear applications. That is the published application for the grade and it follows directly from the chemistry: cobalt and tantalum are held down because both activate under irradiation, and there is no other reason to pay for those extra limits. Typical forged parts we are asked for include valve bodies and bonnets, flanges and nozzle forgings, pump shafts and wear rings, tube sheets, closure rings and support hardware.

Testing and Certification

Each heat is supplied with a mill certificate to EN 10204 3.1. Independent third-party inspection to 3.2 is arranged on request, with the inspection body named on the purchase order. Standard scope covers ladle and product analysis, tensile and elongation at room temperature, hardness, solution treatment record with temperature and quench medium, and dimensional report. Available on request: intergranular corrosion testing to ASTM A262, ultrasonic examination, liquid penetrant examination, Charpy impact at a stated temperature, grain size, and positive material identification.

Questions We Get Asked

What is the difference between AISI 348 and AISI 347?
Both are columbium-stabilized 18Cr-8Ni austenitic steels and the base chemistry is close enough that the two often test alike. The difference in the specification is that A182 Grade F348 lists cobalt at 0.20 % max and tantalum at 0.10 % max. Those two elements activate under neutron irradiation, which is why 348 appears on nuclear prints. If the print does not restrict cobalt, 347 will normally do the job at lower cost.
Can AISI 348 forgings be hardened?
No. Grade 348 does not react to heat treatment. The supply condition is solution treated and quenched. Strength above the annealed level can only come from cold reduction, and that reduces ductility.
What is the minimum tensile strength of A182 F348?
515 MPa [75 ksi] tensile and 205 MPa [30 ksi] yield at 0.2 % offset, with 30 % elongation and 50 % reduction of area minimum. Annealed material typically runs higher, around 655 MPa tensile and 275 MPa yield.
Is there a weight limit on A182 F348 forgings?
Yes. ASTM A182 / A182M caps products made to it at 10 000 lb [4540 kg]. Heavier austenitic forgings go to ASTM A965 / A965M or ASTM A336 / A336M.
Which filler metal is used to weld grade 348?
AWS E348 for covered electrodes and ER348 for bare wire. Fusion and resistance welding are both suitable. Oxyacetylene welding is not preferred for this alloy.
What is the European equivalent of AISI 348?
Designation tables for grade 348 list DIN 1.4550, but 1.4550 is the number for X6CrNiNb18-10, which is AISI 347 / UNS S34700. No EN number carries the cobalt and tantalum restrictions that define S34800. Where those limits matter, order against UNS S34800 or ASTM A182 F348 and do not accept a 1.4550 certificate as equivalent.
What forms can you forge in 348?
Seamless rolled rings, flanges and fittings, shafts and spindles, discs and blanks, tube sheets, sleeves, bushings, bored hollows, and forged bar. Send a drawing, or the grade with outside diameter, inside diameter, length or thickness, and quantity.

Request a Quotation on AISI 348 Forgings

Drawings, a grade and a size, or just the ASTM designation. We reply with price, weight, lead time and the test scope included.

sales@steelforgepieces.com 0086-189-2135-9659

Jiangyin Jiangnan Metal Co., Ltd. · Open-die forging factory · No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Composition and mechanical minima for ASTM A182 / A182M Grade F348 per published specification tables for UNS S34800. Typical annealed properties, physical data, hot working, annealing, machining and welding practice per AZoM grade 348 datasheet. Weight ceiling of 10 000 lb [4540 kg] per the scope of ASTM A182 / A182M. The figures above are for reference; the governing document is the edition of the standard named on your purchase order. Page reviewed 30 September 2026.