Material datasheet / Martensitic stainless steel
ASTM A182 F6B Forgings UNS S41026 · 13 % chromium, 0.5 % molybdenum martensitic stainless steel
ASTM A182 Grade F6B is a martensitic stainless steel forging grade containing 11.5 to 13.5 % chromium, 0.40 to 0.60 % molybdenum and 1.00 to 2.00 % nickel. It is supplied hardened and tempered to 110 to 135 ksi (760 to 930 MPa) tensile strength, 90 ksi (620 MPa) minimum yield strength and 235 to 285 HBW. Jiangyin Jiangnan Metal melts and forges F6B in one works, so the certificate traces back to the melt number rather than to a purchased billet.
- UNS
- S41026
- Family
- Martensitic stainless, hardenable, magnetic
- Cr / Mo / Ni
- 11.5–13.5 % / 0.40–0.60 % / 1.00–2.00 %
- Tensile
- 110–135 ksi
- Yield min
- 90 ksi
- Hardness
- 235–285 HBW
- Also called
- SA-182 F6B, 13Cr-0.5Mo
Grade family
F6B is regularly listed on trade sites as a super-austenitic or 6Mo stainless steel. That description is wrong, and it leads to the grade being specified for duties it cannot survive.
F6B is martensitic. With 11.5 to 13.5 % chromium and only 1.00 to 2.00 % nickel there is nowhere near enough nickel to hold austenite at room temperature, so the structure transforms on cooling and the grade is magnetic and hardenable. Strength comes from the quench and temper, not from alloy content, and its corrosion resistance sits well below the austenitic, duplex and 6Mo families.
If the enquiry mentions seawater, desalination, flue gas desulphurisation or pulp and paper digesters, F6B is the wrong grade. Those duties belong to A182 F44, F51, F53 or the nickel alloys. We forge all of them, and we will say so at quotation stage rather than ship a grade that will not last in the service.
Chemical composition
| Element | Limit | Purpose |
|---|---|---|
| Carbon | 0.15 max | Hardenability and tempered strength |
| Manganese | 1.00 max | Deoxidation and sulphur control |
| Phosphorus | 0.020 max | Held low against temper embrittlement |
| Sulphur | 0.020 max | Held low for transverse toughness |
| Silicon | 1.00 max | Deoxidation |
| Nickel | 1.00 – 2.00 | Hardenability and toughness above plain 13Cr |
| Chromium | 11.5 – 13.5 | Passive film and corrosion resistance |
| Molybdenum | 0.40 – 0.60 | Temper resistance and localised corrosion |
| Copper | 0.50 max | Residual limit |
| Iron | Balance | About 81.2 to 87.1 % |
Values are maxima unless a range is shown. Chemistry is verified at the furnace on site by optical emission spectrometry to ASTM E415.
Mechanical requirements
| Property | Imperial | Metric |
|---|---|---|
| Tensile strength | 110 – 135 ksi | 760 – 930 MPa |
| Yield strength, min | 90 ksi | 620 MPa |
| Elongation in 2 in. [50 mm] or 4D, min | 16 % | 16 % |
| Reduction of area, min | 45 % | 45 % |
| Brinell hardness | 235 – 285 HBW | about 22 – 30 HRC |
Physical and engineering data
| Property | Value |
|---|---|
| Elastic (Young's) modulus | 190 GPa (28 × 106 psi) |
| Shear modulus | 76 GPa (11 × 106 psi) |
| Shear strength | 530 MPa (76 × 103 psi) |
| Fatigue strength | 440 MPa (63 × 103 psi) |
| Poisson's ratio | 0.28 |
| Thermal conductivity | 25 W/m·K (14 BTU/h·ft·°F) |
| Thermal expansion | 10 µm/m·K |
| Specific heat capacity | 480 J/kg·K |
| Melting range | 1400 – 1450 °C |
| Maximum temperature, corrosion | 390 °C (730 °F) |
| Maximum temperature, mechanical | 750 °C (1390 °F) |
| Electrical conductivity | 2.8 % IACS |
| Magnetic response | Ferromagnetic |
Delivery condition and heat treatment
F6B is hardenable, so the delivery condition decides the properties received. ASTM A182 permits liquid quench followed by tempering for martensitic grades. The austenitising and tempering cycle is set out in the heat treatment table of the standard, and we work to the edition named on the purchase order.
| Condition | Yield MPa | Tensile MPa | Elong. | Hardness | Used for |
|---|---|---|---|---|---|
| Annealed | 320 | 540 | 28 % | 175 HB | Rough machining and deep hole drilling before final quench and temper. Not a code delivery condition for F6B. |
| Normalised and tempered | 600 | 780 | 20 % | 24 HRC | Air cooled route for heavy sections where oil quenching risks cracking. |
| Quenched and tempered | 660 | 810 | 20 % | 26 HRC | Standard condition for F6B flanges, valve bodies and fittings. Meets the 110 ksi and 90 ksi minimums. |
| Quenched and tempered, high strength | 800 | 950 | 16 % | 31 HRC | Where the part must match a 130 ksi class body or trim. |
Several datasheets in circulation quote an anneal at 2100 to 2150 °F with a water quench for F6B. That is a solution anneal belonging to super-austenitic grades. Applied to a 13Cr martensitic forging it would leave the part far outside the specified strength and hardness band. Our process sheets follow the A182 heat treatment table only.
Corrosion behaviour and limits
F6B forms a passive chromium oxide film and gives useful service in fresh water, steam, dry gas, crude oil and mild organic media. Molybdenum improves temper resistance and localised corrosion behaviour compared with plain 13Cr, and nickel raises hardenability and toughness compared with A182 F6A.
The limits matter as much as the strength. Published data puts the maximum corrosion service temperature at about 390 °C. With 13 % chromium and 0.5 % molybdenum this is not a chloride or seawater material. Pitting in chloride-bearing media and cracking risk at the upper end of the hardness band are the two failure modes to design against.
Sour service, NACE MR0175 and ISO 15156
F6B can go into sour service only on a restricted hardness specification. A general 22 HRC limit applies to many materials in H2S-bearing service, which sits at the bottom of the 235 to 285 HBW band F6B is normally supplied to, so much of the standard range is above the general cap. Certain martensitic stainless steels are allowed higher limits under specific clauses of the standard, which is why the environment has to be defined before the material is released.
Send the H2S partial pressure, temperature, chloride concentration and in-situ pH with the enquiry. We then set the hardness cap, the heat treatment and the test plan against the correct selection table.
Grade comparison
| Grade | UNS | Family | Cr / Mo / Ni | Strength | Role |
|---|---|---|---|---|---|
| F6B | S41026 | Martensitic | 11.5–13.5 / 0.40–0.60 / 1.0–2.0 | 110–135 ksi | Trim, stems, high strength flanges |
| F6A | S41000 | Martensitic | 13Cr, no specified Mo | 70–130 ksi by class | General 13Cr fittings |
| F6NM | S41500 | Soft martensitic | 13Cr / Mo / 4Ni | — | Where weld and impact toughness govern |
| F51 | S31803 | Duplex | 22Cr / 3Mo / 5Ni | — | Chloride-bearing process duty |
| F53 | S32750 | Super duplex | 25Cr / 4Mo / 7Ni | — | Seawater and subsea |
| F44 | S31254 | Super-austenitic 6Mo | 20Cr / 6Mo / 18Ni | — | Seawater, FGD, desalination |
What we forge in F6B
Valve and wellhead parts
Bodies, bonnets, stems, seat rings, plugs, gates and wedges for ball, gate, globe, check and plug valves in non-chloride service.
Forged flanges
Weld neck, blind, slip-on, socket weld, lap joint and orifice flanges to ASME B16.5, B16.47 and API 6A dimensions.
Seamless rolled rings
Radial-axial rolled rings from OD 50 mm to OD 6,000 mm, for bearing carriers, retaining rings and pressure boundary blanks.
Shafts and bars
Pump and compressor shafts, spindles, stems and tie rods, turned to 14,000 mm between centres, quenched vertically in the 15 m well furnaces.
Discs and tube sheets
Solid forged discs, covers and tube sheet blanks to 5,000 mm machined diameter, supplied proof-machined for volumetric inspection.
Sleeves and bushings
Wear sleeves, bushings, liners and bored cylinders to 1,600 mm diameter by 10,000 mm on the deep-hole drilling machine.
Fabrication notes
Forging
Hot work in the usual martensitic stainless range and finish above the point where the grade begins to harden on cooling, then slow cool or anneal straight away so untempered martensite does not crack the piece. The forging is cooled below the temperature set in A182 before the specified heat treatment is applied.
Machining
Rough machine in the annealed condition wherever the drawing allows, then finish after quench and temper. In the hardened condition use rigid setups, sharp carbide tooling and heavy positive feeds so the tool cuts under the work-hardened layer instead of glazing it.
Welding
Weldable with care because of the martensitic structure. Normal practice is preheat with a controlled interpass temperature, a matching 13Cr or 13Cr-4Ni filler, or an austenitic filler where softer weld metal is acceptable, followed by a post-weld temper to soften the heat affected zone. Where weld toughness governs the design, F6NM is the usual alternative.
Manufacturing and quality
Steel for F6B is melted on site rather than bought in as billet, so the chemistry can be aimed at the forging it will become and the certificate traces back to the melt number.
| Step | Capability |
|---|---|
| Melting | 25 t electric arc furnace, 25 t and 50 t ladle furnaces, 30 t and 60 t vacuum oxygen decarburisation. Maximum heat size 60 t. Electroslag remelting available where cleanliness governs. |
| Forging | 6,300 t, 4,000 t and 2,000 t hydraulic open-die presses. Hammers from 750 kg to 5 t. Maximum single piece 30 t. |
| Ring rolling | Radial-axial mills at 6 m, 3 m and 1 m. Maximum outside diameter 6,000 mm, minimum from OD 50 mm by the upset and punch route. |
| Heat treatment | 14 furnaces. Car-bottom chambers to 8,000 × 2,000 × 2,000 mm and two well-type furnaces 15,000 mm deep for vertical quenching of long shafts. |
| Machining | Vertical lathes to 5,000 mm swing, horizontal lathes to 14 m, CNC machining to 2,000 mm diameter by 10,000 mm, CNC deep-hole drilling to 1,600 mm by 10,000 mm. |
| Chemistry | Optical emission spectrometry to ASTM E415, infrared carbon and sulphur to ASTM E1019, handheld PMI. |
| Mechanical testing | 600 kN and 300 kN universal testing machines to ASTM A370 and ISO 6892. Charpy V-notch with low temperature bath to −60 °C. |
| Ultrasonic testing | ASTM A388 and EN 10228-3 on full-digital equipment. Magnetic particle to ASTM E709. Grain size to ASTM E112. |
| Approvals | CCS, BV, DNV, LR and NK. |
| Certification | EN 10204 3.1 mill certificate, or EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer's own inspector. |
| Order terms | Minimum order 10 kg, no minimum piece count. Normal lead time 20 to 60 days. |
Grade and edition (ASTM A182 F6B or ASME SA-182 F6B), the drawing or rough dimensions, the quantity, the delivery condition, the heat treatment and testing requirements, the certificate level and the destination port. If the duty is sour or chloride bearing, add the service conditions. Email sales@steelforgepieces.com or call +86 189 2135 9659. Quotations normally go out within two working days.
Frequently asked questions
Is ASTM A182 F6B austenitic or martensitic?
Martensitic. UNS S41026 carries 11.5 to 13.5 % chromium with only 1.0 to 2.0 % nickel, far below what is needed to hold austenite at room temperature. It is magnetic and hardenable by heat treatment. Listings that call it super-austenitic or 6Mo are incorrect.
What is the difference between A182 F6A and A182 F6B?
F6A is UNS S41000, close to forged Type 410, with no specified molybdenum. F6B is UNS S41026 and adds 0.40 to 0.60 % molybdenum and 1.00 to 2.00 % nickel, with phosphorus and sulphur both held to 0.020 % maximum. F6A is supplied in several strength classes. F6B has one level at 110 to 135 ksi tensile and 235 to 285 HBW.
What are the mechanical properties of F6B?
Tensile 110 to 135 ksi (760 to 930 MPa), yield 90 ksi (620 MPa) minimum, elongation 16 % minimum in 2 in. or 4D, reduction of area 45 % minimum, hardness 235 to 285 HBW.
Can F6B be used in seawater or a desalination plant?
No. It is a 13 % chromium grade with 0.5 % molybdenum and a published maximum corrosion service temperature of about 390 °C, and it will pit in chloride-bearing water. Use F44, F51 or F53 for those duties. We forge all three.
Is F6B acceptable under NACE MR0175 and ISO 15156?
Conditionally, on a restricted hardness specification. The general 22 HRC sour service limit sits at the bottom of the standard 235 to 285 HBW band, so restricted hardness heat treatment and hardness testing must be specified at order. Supply the H2S partial pressure, temperature, chloride level and pH with the enquiry.
Is UNS S41026 the same material as A182 F6B?
Yes. S41026 is the UNS designation for A182 Grade F6B. The ASME pressure vessel designation is SA-182 F6B.
What is the largest F6B forging you can produce?
Seamless rings roll to 6,000 mm outside diameter on the 6 m radial-axial mill, with 3 m and 1 m mills for smaller sizes. The heaviest single forging is 30 tonnes, worked on 6,300 t, 4,000 t and 2,000 t presses, and maximum heat size in the melt shop is 60 tonnes. Minimum order is 10 kg with no minimum piece count.
Do you supply finish-machined F6B parts or rough forgings only?
Both. Parts can be supplied as-forged with machining allowance, rough-machined to a proof-machined condition suitable for ultrasonic testing, or finish-machined to drawing. Heat treatment, machining and testing are carried out on site.
Sources and scope
Composition and mechanical requirements are those of ASTM A182/A182M for Grade F6B, UNS S41026. Physical property values are published reference data for the annealed condition. Delivery condition property levels are published supplier data. Sour service limits follow NACE MR0175 and ISO 15156. Dimensional and equipment figures are this plant's own capability. Buyers should verify all values against the current edition of the governing standard. Nothing on this page is a material certification.