GRADE 1.4841 / X15CrNiSi25-21 / AISI 314 / UNS S31400 MELTED AND FORGED IN ONE WORKS, JIANGYIN, CHINA +86 189 2135 9659 · sales@steelforgepieces.com
Jiangyin Jiangnan Metal Open-die forging and ring rolling, since 1997 Get a quote

Heat resistant steel forgings to EN 10095

1.4841 Forgings X15CrNiSi25-21, AISI 314, UNS S31400, BS 314S25. Forged rings, flanges, bars, shafts, discs and tube sheets, scale resistant in air to about 1150 C.

1.4841 is the EN material number for X15CrNiSi25-21, a fully austenitic 25 percent chromium, 20 percent nickel heat resistant steel with a silicon addition that raises its scaling resistance in air to roughly 1150 C. Jiangyin Jiangnan Metal melts the grade in-house and forges it to drawing, so the certificate traces the part to its own heat number rather than to a purchased billet.

Send a drawing   Go to composition

01

Grade identity

1.4841 / X15CrNiSi25-21 is a fully austenitic chromium nickel silicon steel standardised in EN 10095 for heat resisting service. Chromium of 24.0 to 26.0 percent and nickel of 19.0 to 22.0 percent give the austenitic structure and the chromia forming base. The silicon addition of 1.5 to 2.5 percent is the defining feature, because it stabilises and thickens the protective oxide and lowers oxidation rates in the 900 to 1100 C window compared with a plain 310 type steel at the same chromium and nickel level.

Two limits govern selection. Scaling resistance and load carrying capacity are separate properties: the grade resists scaling in air to about 1150 C, while creep resistance runs out at roughly 690 C, so pressure retaining and load bearing parts are designed to creep data rather than to the oxidation limit. The grade also must not be held in the 600 to 900 C band during processing, because sigma phase embrittlement forms there.

Designation note. 1.4841 is sometimes listed in trade catalogues as 310H. AISI 310H is UNS S31009, the high carbon variant of the 310 and 310S family, and its EN number is 1.4845. 1.4841 maps to AISI 314 / UNS S31400. Some equivalence tables also cross reference 1.4841 to AISI 310 / UNS S31000 because the chromium and nickel bands overlap, but the silicon content does not, and the two grades behave differently in sulphur bearing and thermally cycled service. State the governing standard on the purchase order and the grade is confirmed against the drawing before quotation.
02

Equivalent and related grades

An equivalent means comparable chemistry and comparable typical properties, not an identical specification. Where a national grade differs on silicon, nickel or carbon, the difference is given.

1.4841 / X15CrNiSi25-21 cross references
SystemDesignationNote
EN 10095X15CrNiSi25-21, 1.4841Governing designation on this page
SEW 470X15CrNiSi25-20, 1.4841Same number, nickel band 19.0 to 21.0 percent
ASTM, UNS, SAEAISI 314, UNS S31400, SAE 314Primary US cross reference, silicon bearing
ASTM, UNS (loose)AISI 310, UNS S31000Listed commercially. Silicon 1.5 percent maximum only, so not interchangeable in cycling or sulphur service
BS314S25
JISSUH 310
AFNORZ15CNS25-20Carbon 0.15 percent maximum
GOST20Ch25N20S2Silicon 2.0 to 3.0 percent, chromium 24.0 to 27.0 percent
PNH25N20S2, H25N20S25Silicon 2.0 to 3.0 percent
UNEF-3310
CSN17255
DIN, olderX16CrNiSi25-20, 1.2782Silicon 1.8 to 2.3 percent

Neighbouring grades from the same works

1.4845, 310S and 310H

X12CrNi25-21 and X8CrNi25-21. Carbon is lower than in 1.4841 and published comparisons credit the grade with better scaling resistance on that account. Specified where the assembly is welded and intergranular attack is a concern. 310H, UNS S31009, is the high carbon creep variant of the same family.

1.4828, AISI 309

X15CrNiSi20-12. The same chromium nickel silicon concept at a lower alloy level, heat resistant to roughly 950 to 1000 C. Used where 1150 C capability is not required.

Incoloy 800H, 800HT and Alloy 330

Where creep strength above roughly 700 C governs the design rather than oxidation alone, the nickel iron chromium alloys replace 1.4841. Both families are forged in this works. See the nickel alloy index.

03

Chemical composition

Weight percent, balance iron. Ladle analysis and product analysis are both reported on the mill certificate against the heat number. Published data sheets differ on the silicon band according to the standard cited, so both are given. State the requirement at enquiry and it is written into the melt instruction.

1.4841 chemical composition, percent by weight
ElementSymbolEN 10095Per EN 10088-3 data sheets
CarbonC0.20 max0.20 max
SiliconSi1.50 to 2.501.50 to 2.00
ManganeseMn2.00 max2.00 max
PhosphorusP0.045 max0.045 max
SulphurS0.015 max0.015 max
NitrogenN0.11 max0.11 max
ChromiumCr24.0 to 26.024.0 to 26.0
NickelNi19.0 to 22.019.0 to 22.0
IronFeBalanceBalance

Molybdenum, titanium, niobium, aluminium, vanadium and copper are not alloyed additions in 1.4841. They are treated as residuals and can be restricted below the table values where a specification requires it.

04

Mechanical, physical and creep data

Room temperature values apply to the solution annealed condition to EN 10095 for diameters up to about 160 mm. Contractual values are those agreed at order and certified for the delivered heat and section size.

Room temperature mechanical properties, solution annealed
PropertyValue
Tensile strength, Rm550 to 750 MPa
Yield strength, Rp0.2230 MPa minimum
Yield strength, Rp1.0270 MPa minimum
Elongation A5, longitudinal30 percent minimum, published practice 28 percent minimum
Hardness223 HB maximum
Magnetic responseNon-magnetisable, slightly magnetic after cold work
PREN24.0 to 29.3
Physical properties
PropertyValue
Density at 20 C7.9 kg/dm3
Thermal conductivity at 20 Capprox. 15 W/(m K)
Specific heat, 20 to 100 C500 J/(kg K)
Electrical resistivity at 20 C0.90 ohm mm2/m
Electrical resistivity at 1000 C1.25 ohm mm2/m
Mean thermal expansion, 20 to 100 C15.0 to 15.2 x 10-6/K
Mean thermal expansion, 20 to 500 C17.0 x 10-6/K
Mean thermal expansion, 20 to 800 C18.0 x 10-6/K
Mean thermal expansion, 20 to 1000 C19.0 x 10-6/K
Mean thermal expansion, 20 to 1200 C19.5 x 10-6/K

Creep rupture strength and creep limit

Published creep data for X15CrNiSi25-21. This is the data set used for any part carrying load at temperature, and it explains why a 1150 C oxidation rating does not give a 1150 C service part.

Creep rupture strength and 1 percent creep limit, MPa
TemperatureRz/1000Rz/10000Rz/100000R1/1000R1/10000
600 C1701308010595
700 C9040185035
800 C402072310
900 C20103104
1000 C53
05

Service limits by atmosphere

A single maximum service temperature for a heat resistant steel assumes clean oxidising air. Furnace, refinery and process atmospheres shift the limit, in some cases by 400 C or more.

Service limits for 1.4841
ConditionLimitGoverning mechanism
Scaling resistance, air, isothermalapprox. 1150 CChromium silicon oxide stability
Sustained practical service, airapprox. 1100 CScale growth and grain coarsening
Thermally cycled serviceBelow the continuous figureScale spalls on cooling, metal loss per cycle rises
Load bearing and creep dutyapprox. 690 CCreep strength, see creep table
Oxidising and reducing sulphurous gasesapprox. 650 CNickel sulphur attack
Nitrogenous, carburising, low oxygen gasesapprox. 900 C, medium resistanceNitriding and carburisation
Range to avoid600 to 900 CSigma phase embrittlement
Cycled duty. Furnace fixtures, retort covers and burner hardware that heat and cool daily lose scale at every cooldown, which resets the protective layer and consumes metal faster than an isothermal test predicts. State the cycle at enquiry: temperature, dwell, cycles per day and atmosphere. On strongly cycled, sulphur bearing or carburising duty an Incoloy 800H, 800HT or Alloy 330 forging may give longer life than 1.4841, and both families are forged here.
06

Melting, forging, heat treatment and fabrication

Melting route

1.4841 is melted in the 25 t electric arc furnace, refined in a 25 t or 50 t ladle furnace and vacuum oxygen decarburised at 30 t or 60 t. That route brings a 25 percent chromium steel to a controlled carbon and nitrogen level without losing chromium to the slag. Protective atmosphere electroslag remelting at 3 t or 6 t is added where an order calls for tighter cleanliness and lower centreline segregation. Maximum heat size is 60 t.

Forging

Open-die forged on 6,300 t, 4,000 t and 2,000 t hydraulic presses, or ring rolled on 6 m, 3 m and 1 m radial-axial mills, with 5 t, 3 t, 2 t, 1 t and 750 kg hammers for drawing out and small batch work. The forging window runs from roughly 1175 C down to 1000 C with rapid cooling in air or water afterwards, and secondary hot forming is carried out between about 1150 C and 800 C. The grade forges well, and because the window is narrow and the sigma phase band sits directly below it, the reheating schedule is planned per part.

Heat treatment practice for 1.4841 forgings
OperationTemperatureCoolingPurpose
Forging1175 to 1000 CRapid, air or waterShape the part and break down the as-cast structure
Hot forming1150 to 800 CAirSecondary shaping operations
Solution annealing1050 to 1150 CAir or waterDissolve carbides and restore homogeneous austenite
Avoid600 to 900 C holdSigma phase embrittlement

1.4841 is not age hardened. It is an austenitic heat resistant steel rather than a precipitation hardening steel, so no solution plus ageing cycle applies, and strength at temperature comes from the matrix and the alloy content. Solution annealing is carried out in one of 14 furnaces on site, including three high temperature car bottom furnaces, and the time and temperature chart is supplied with the certificate.

Welding in downstream fabrication

Forgings from this works are produced from solid, so the delivered part contains no weld. For customer fabrication, 1.4841 suits TIG, MAG, submerged arc, laser and manual arc welding and normally requires no preheat and no post weld heat treatment. The grade is prone to hot cracking, so welding energy is limited, and 1.4842, which is X12CrNi25-20, is a commonly used filler. Corrosion resistance is reduced by welding and the as welded material is susceptible to intergranular corrosion, which is one reason heavily welded assemblies are sometimes specified in the lower carbon 1.4845.

Machining

Machinability is medium. Carbides forming during cutting accelerate tool wear, and low thermal conductivity combined with a strong work hardening tendency calls for light depth of cut, reduced cutting speed and generous coolant. Parts can be ordered as forged with allowance, proof machined for ultrasonic inspection, or finish machined to drawing.

07

Forged product forms in 1.4841

Each item is forged to drawing from one piece of steel melted on site, with no welding and no casting. Shapes outside this list are quoted the same way.

Seamless rolled rings

1.4841 seamless and contoured rolled rings, rectangular or profiled section, for furnace fixtures, burner grids, slewing and bearing applications.

Forged rings

1.4841 forged rings, retaining rings, gear rings and valve seat rings for sections outside the ring mill envelope or where heavy reduction is specified.

Forged flanges

1.4841 weld neck, blind, slip-on, socket weld, lap joint, orifice, anchor, girth, swivel and long weld neck flanges to ASME B16.5 and B16.47 dimensions.

Forged bars and blocks

1.4841 forged round bars, flat bars, square bars and blocks, used as feedstock for machined bodies, hangers and tooling.

Forged shafts

1.4841 shafts, spindles, eccentric shafts, rolls and walking beam components for furnace and thermal processing plant.

Discs and tube sheets

1.4841 solid and bored discs, tube sheets, covers and hubs for heat exchangers and pressure vessels, supplied proof machined for volumetric inspection.

Sleeves, bushings and cylinders

1.4841 forged sleeves, bushings, couplings, hollow cylinders and heavy wall pipe sections bored from solid forged blanks.

Valve and nozzle parts

1.4841 valve bodies, bonnets, blocks, stems, seat rings, spools, nozzles and manifolds for high temperature service.

Works envelope, outer limits for a 1.4841 forging
FormLimitSet by
Seamless rolled ringsto 6,000 mm outside diameter6 m radial-axial ring mill
Minimum ringfrom 50 mm outside diameterUpset and punch route below ring mill range
Shaftsto 14,000 mm turned lengthC61160 lathe, 15 m well furnace for vertical quench
Discs, tube sheets, blocksto 5,000 mm machined diameter5,000 mm vertical turning lathe
Bored cylinders, hollow shaftsto 1,600 mm diameter by 10,000 mmCNC deep hole drilling machine
Single piece weightto 30,000 kg60 t heat size, 6,300 t press
Minimum order10 kg, no minimum piece countCommercial policy

These are plant limits rather than grade limits. For a given 1.4841 part the practical maximum also depends on shape and on the forging reduction ratio required, so the drawing is reviewed before a size is confirmed.

08

Testing, approvals and certification

Chemistry is verified at the furnace rather than taken from a supplier certificate, and traceability runs from the melt number through forging, heat treatment and machining to shipment.

Non-destructive testing

NDT performed on 1.4841 forgings
MethodStandardEquipment
Ultrasonic testingASTM A388, EN 10228-3 or SEP 1921, to the class on the orderPXUT-3300, USM35XS, CTS-22
Liquid penetrantSurface examination, used in place of MPI on austenitic material
Magnetic particleASTM E709 or customer procedure, where the grade condition permitsCYE-3A
Bore inspectionVisual examination of boresDNJ industrial endoscope

1.4841 is fully austenitic and is not magnetisable in the annealed condition, so magnetic particle inspection is generally not applicable and liquid penetrant is used for surface examination. EN 10228-3 addresses ferritic and martensitic forgings, so for austenitic material the ultrasonic procedure and acceptance class are agreed case by case, usually against ASTM A388 with a stated reference reflector. Agree this at enquiry stage rather than at inspection.

Chemical and mechanical testing

In-house laboratory scope
DisciplineEquipmentStandard
Chemical analysisSPECTROTEST TXC25 optical emission spectrometerASTM E415
Carbon and sulphurHIR-9440D infrared analyserASTM E1019
Alloy verificationX-Mwt3000TX handheld analyserPositive material identification
TensileWE-600B 600 kN, WDW-300ASTM A370, ISO 6892
ImpactJBN-300 with DWC-60 low temperature bathASTM A370, to minus 60 C
HardnessTH140 Leeb testerASTM A956, converted per ASTM E140
MetallographyXJP-6A microscope, mounting press, polisherASTM E112 grain size

Tests outside that scope are placed with an accredited third party laboratory and the report is issued alongside the mill certificate. This covers intergranular corrosion to ASTM A262 or ASTM G28, pitting to ASTM G48, impact testing below minus 60 C, and bench Brinell or Rockwell hardness where the specification calls for a fixed machine rather than a portable instrument. State the requirement on the enquiry so that it is scheduled before shipment.

Approvals and documents

Certification for 1.4841 forgings
ItemDetail
Class approvals heldCCS, BV, DNV, LR, NK
Standard certificateEN 10204 3.1 mill test certificate
Witnessed certificateEN 10204 3.2, witnessed by BV, DNV, LR, SGS, TUV or the customer inspector, on request
TraceabilityMelt number through forging, heat treatment and machining to shipment
Supporting recordsHeat treatment charts, UT reports, dimensional reports, PMI records
09

Applications

Typical applications for 1.4841 and AISI 314 forgings
SectorParts
Furnace and thermal processingAnnealing covers and boxes, burner grids and shields, retort and muffle components, doors, fan hubs, walking beams, recuperator parts, conveyor components and hooks
Steel, smelting and sintering plantFluidised bed furnace internals, coal combustor grids, wind box components, burners, feeding and discharging hardware, continuous casting equipment
Refining and petrochemicalCatalytic recovery system parts, flare components, recuperators, tube hangers, FCC unit hardware, gas pyrolysis and methane conversion equipment
Pressure equipmentTube sheets, covers, flanges and shell components for high temperature shell and tube heat exchangers, columns, towers, preheaters and silos
Glass, ceramics and cementBlowpipe ends, porcelain baskets and carriers, conveyor components, kiln and cooler hardware
Valves for hot serviceValve bodies, bonnets, stems, seat rings and nozzles operating above the range of standard austenitic grades
10

Request a quotation

Quotations are prepared from a drawing or a written specification. Sending the items below in the first email removes a round trip and normally returns a price within two working days. Minimum order is 10 kg with no minimum piece count, and normal lead time for 1.4841 is 20 to 60 days.

What to include in a 1.4841 enquiry
ItemDetail requiredExample
1Grade and governing standard1.4841 to EN 10095, or AISI 314 / UNS S31400
2Dimensions, or a drawing in PDF, DWG, DXF or STEP1200 mm OD by 900 mm ID by 260 mm high
3Quantity and expected repeat volume12 pieces, about 4 per year
4Delivery conditionSolution annealed, proof machined
5Service conditions980 C, cycled twice daily, oxidising, low sulphur
6Testing, certification and destination portUT to ASTM A388, EN 10204 3.2 witnessed by DNV, Rotterdam

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
+86 189 2135 9659 · sales@steelforgepieces.com
Email the works

11

Questions about 1.4841

What is 1.4841 steel?

1.4841 is the EN material number for X15CrNiSi25-21, a fully austenitic chromium nickel silicon heat resistant steel to EN 10095 with 24.0 to 26.0 percent chromium, 19.0 to 22.0 percent nickel, carbon to 0.20 percent and silicon of 1.5 to 2.5 percent. The silicon separates it from plain 310 type steel, since it stabilises the protective oxide and gives scaling resistance in air to about 1150 C. Jiangyin Jiangnan Metal forges the grade to drawing as rings, flanges, bars, shafts, discs, tube sheets, sleeves and valve parts.

Is 1.4841 the same as AISI 310H?

No. 1.4841 corresponds to AISI 314 and UNS S31400. AISI 310H is UNS S31009, the high carbon variant of the 310 and 310S family, with the EN number 1.4845. 1.4841 is cross referenced to AISI 310 and UNS S31000 in some commercial tables because the chromium and nickel bands overlap, but the silicon content differs. State the governing standard on the purchase order. This works forges 1.4841, 1.4845 and 1.4828 and confirms which grade matches the drawing.

What is the chemical composition of 1.4841?

To EN 10095: carbon 0.20 percent maximum, silicon 1.50 to 2.50 percent, manganese 2.00 percent maximum, phosphorus 0.045 percent maximum, sulphur 0.015 percent maximum, nitrogen 0.11 percent maximum, chromium 24.0 to 26.0 percent, nickel 19.0 to 22.0 percent, balance iron. Data sheets citing EN 10088-3 give a narrower silicon band of 1.50 to 2.00 percent. Ladle and product analysis are both reported on the mill certificate against the heat number.

What is the maximum service temperature of 1.4841?

Scale resistant in air to approximately 1150 C, with sustained practical service closer to 1100 C. Creep resistance is the earlier limit for loaded parts, at roughly 690 C. In oxidising and reducing sulphurous gases the limit is about 650 C, and resistance to nitrogenous, carburising and low oxygen gases is medium up to about 900 C. Cyclic duty lowers the useful limit below the continuous figure, because scale spalls at each cooldown.

In what condition are 1.4841 forgings supplied?

Solution annealed at 1050 to 1150 C, cooled in air or water. 1.4841 is not a precipitation hardening steel, so no ageing treatment applies. Hot forming runs between about 1150 C and 800 C, and the 600 to 900 C band is avoided because of sigma phase embrittlement.

Which forged shapes are available in 1.4841?

Seamless and contoured rolled rings, forged rings and retaining rings, weld neck, blind, slip-on and long weld neck flanges, round, flat and square bars, shafts and spindles, solid and bored discs, tube sheets and covers, sleeves, bushings, hollow cylinders, heavy wall pipe bored from solid, and valve bodies, bonnets, stems, seat rings and nozzles. Each item is forged to drawing from one piece of steel melted on site.

How large can a 1.4841 forging be?

To 6,000 mm outside diameter on the 6 m radial-axial ring mill and 30,000 kg for a single forged piece on the 6,300 t press, with 5,000 mm machined diameter for discs and tube sheets, 14,000 mm turned length for shafts and 1,600 mm by 10,000 mm for deep bored cylinders. The minimum ring is about 50 mm outside diameter and the minimum order is 10 kg. The practical limit for a given part also depends on shape and forging reduction, so the drawing is reviewed first.

Can 1.4841 be welded?

Yes. TIG, MAG, submerged arc, laser and manual arc welding are all suitable, normally without preheat or post weld heat treatment. Welding energy is limited because the grade is prone to hot cracking, and 1.4842, which is X12CrNi25-20, is a commonly used filler. Corrosion resistance falls after welding and the as welded material is susceptible to intergranular corrosion, which is why heavily welded assemblies are sometimes specified in the lower carbon 1.4845.

How machinable is 1.4841?

Medium. Carbides forming during cutting accelerate tool wear, and low thermal conductivity with a strong work hardening tendency calls for light depth of cut, reduced speed and generous coolant. Forgings are supplied as forged with allowance, proof machined for ultrasonic inspection, or finish machined to drawing.

What testing and certification is supplied?

Ultrasonic testing to ASTM A388, EN 10228-3 or SEP 1921 at the agreed class, liquid penetrant examination, optical emission spectrometry, positive material identification, tensile and hardness testing, dimensional inspection and grain size on request. EN 10204 3.1 as standard, EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer inspector on request. The works holds CCS, BV, DNV, LR and NK approvals.

What is the lead time?

20 to 60 days from order confirmation. Standard heat resistant grades such as 1.4841 sit at the lower end, since they run through the electric arc furnace and VOD without a remelting step. Witnessed 3.2 inspection and outside laboratory corrosion testing require scheduling, so state both at enquiry.

Can the works be visited or audited?

Yes. The plant is at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China, between Shanghai and Nanjing on the south bank of the Yangtze. Wuxi Shuofang International Airport is about 30 km away and the Shanghai airports about 160 km. Customer audits and third party inspections are welcome. Email sales@steelforgepieces.com or call +86 189 2135 9659.

12

Standards and sources

Composition, property, temperature and heat treatment data on this page are taken from the standards and published data sheets below. Where sources differ, notably on the silicon band and on the practical against nominal temperature limit, both figures are given in the tables above.

References
ReferenceUsed for
EN 10095Grade definition, composition limits, solution annealed mechanical properties
EN 10088-3Alternative silicon band quoted by published data sheets
SEW 470, NF A35-573, UNE 36017, GOST, PN, BS, JISNational equivalence and designation cross references
ASTM A388, EN 10228-3, SEP 1921Ultrasonic examination of forgings
EN 10204Inspection document types 3.1 and 3.2
ASTM A370, ISO 6892, ASTM E112, E415, E1019, E709, A956, E140Mechanical, chemical and NDT test methods used in the in-house laboratory

Published by Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Page last reviewed 26 September 2026. Data is given for reference and design guidance. Contractual values are those agreed at order and certified for the delivered heat. Telephone +86 189 2135 9659, email sales@steelforgepieces.com.