UNS C71500 70/30 copper-nickel. Open-die forged tubesheets, rings, flanges, discs and bars.
C71500 is the higher-nickel half of the marine cupronickel pair. Where 90/10 runs out of velocity headroom or meets water that is warm, polluted or sandy, 70/30 is what the specification usually moves to. This page carries the composition and property data a fabricator needs to check a drawing against, plus what we can forge, test and certify.
Grade at a glance
- UNS number
- C71500
- Nominal composition
- Cu 70, Ni 30
- Plate and tubesheet spec
- ASTM B171 / ASME SB-171
- Rod and bar spec
- ASTM B151
- Condition supplied
- Hot forged and annealed
- Tensile minimum, to 60 mm
- 345 MPa (50 ksi)
- Seawater design velocity
- 3.5 to 4.0 m/s, clean water
- Certification
- EN 10204 3.1, 3.2 on request
What is UNS C71500?
C71500 is a wrought copper-nickel carrying 29.0 to 33.0 % nickel, 0.40 to 1.0 % iron and up to 1.0 % manganese, with copper making up the rest. It is a single-phase solid solution. There is no second phase to precipitate and no transformation to quench, which is why the alloy behaves the way it does in every downstream operation: it cannot be hardened by heat treatment, it stays tough down to cryogenic temperature, and it work-hardens steadily rather than suddenly.
The iron is the part people overlook. Iron in solid solution is what gives copper-nickel its resistance to impingement attack in flowing seawater, and it only works while it stays in solution. Iron that has come out as a separate phase, usually through slow cooling from annealing temperature, contributes nothing to corrosion resistance and can act as a local anode. That is the reason annealed copper-nickel is cooled quickly rather than left to cool in the furnace.
Against 90/10 copper-nickel, C71500 buys roughly 25 % more strength, a higher allowable flow velocity, better behaviour in polluted or sulphide-bearing water, and useful strength retention to around 300 degrees C. It gives up about a third of the thermal conductivity and costs more, since nickel dominates the price. Most projects therefore run 90/10 for the bulk piping and specify 70/30 where the duty is hardest, which in a shell and tube exchanger usually means the tubesheet and the tube inlets.
Specifications C71500 forgings are supplied to
Copper-nickel does not have a dedicated forging specification in the way steel has ASTM A182 or A266. Tubesheets, discs and flanges are normally bought to the plate specification, ASTM B171, and bars to ASTM B151, with the forging route and any extra testing written into the order. Naming the standard matters here, because the minor element limits differ between them.
| Standard | Covers | Used for |
|---|---|---|
| ASTM B171 / ASME SB-171 | Copper alloy plate, sheet and rolled bar for condensers and pressure vessels | Tubesheets, tube plates, baffles, support plates, disc blanks |
| ASTM B151 | Copper-nickel rod and bar | Round bar, hexagon, machined blanks, stud and fastener stock |
| ASTM B122 | Plate, sheet, strip and rolled bar | General plate and strip work |
| ASTM B111 / B395 | Seamless condenser and heat exchanger tube | Tube bundles matched to a C71500 tubesheet |
| ASTM B466 / B467 | Seamless and welded pipe | Seawater pipework, water box connections |
| EN 12163 / EN 12420 / EN 1653 | European rod, forgings and plate in CuNi30Mn1Fe | European projects quoting CW354H |
| DIN 17664 / 2.0882 | German copper-nickel wrought products | Older German drawings |
| MIL-T-16420 / DEF STAN | Naval condenser tube and associated components | Naval and minehunter work, where permeability is also specified |
Worth settling at enquiry stage. ASTM B171 tightens zinc, lead, phosphorus, sulphur and carbon when the purchaser specifies that the material is for subsequent welding: zinc 0.50 % max, lead 0.02 % max, phosphorus 0.02 % max, sulphur 0.02 % max and carbon 0.05 % max. If the tubesheet will be seal welded or strength welded to the tubes, say so on the enquiry so the billet is bought against the welding limits rather than the general ones.
Chemical composition of C71500
| Element | Minimum | Maximum | Note |
|---|---|---|---|
| Nickel, including cobalt | 29.0 | 33.0 | Sets strength and corrosion behaviour |
| Iron | 0.40 | 1.0 | Must stay in solid solution to resist impingement |
| Manganese | - | 1.0 | Deoxidiser and strengthener |
| Zinc | - | 1.0 | 0.50 % max when specified for welding |
| Lead | - | 0.05 | Causes hot shortness during forging; 0.02 % max when specified for welding |
| Copper, including silver | Remainder | Balance of the analysis | |
| Copper plus named elements | 99.5 | - | Total of the listed elements |
Two elements do damage far below their nominal limits. Lead and bismuth segregate to grain boundaries and open the forging up at temperature, which is why scrap from unknown sources is not used for this grade. Sulphur does the same thing during heating rather than during deformation. Carbon above roughly 0.05 % is also unwelcome, since it forms a film on grain boundaries that shows up later as poor bend behaviour and porous welds.
Each heat is analysed by optical emission spectrometry, with copper alloy analysis run to ASTM E478 rather than the ASTM E415 method used for steel, and the result is reported against the standard named on the order. Positive material identification with a handheld analyser is carried out on the finished part before despatch when it is asked for.
Mechanical properties of C71500
ASTM B171 sets its minima by thickness, in the hot rolled and annealed tempers. Forged tubesheets are supplied against the same figures. Yield is quoted at 0.5 % extension under load rather than 0.2 % offset, which is standard practice for copper alloys and is worth checking before a design calculation is done against the number.
| Thickness | Tensile strength, min | Yield strength, min 0.5 % extension under load | Elongation in 50 mm, min |
|---|---|---|---|
| Up to 60 mm (2.5 in.) | 345 MPa 50 ksi | 140 MPa 20 ksi | 30 % |
| Over 60 to 140 mm (2.5 to 5 in.) | 310 MPa 45 ksi | 125 MPa 18 ksi | 30 % |
ASTM B151 sets separate minima for rod and bar, stepped by temper and by diameter. Published restatements of that table do not agree with one another, so the row that governs a given order should be read from the standard itself and quoted on the purchase order. We test and certify against whichever row the order names.
Typical results on annealed forged material sit above these minima rather than at them, but the margin is modest. Published typical figures for hot rolled 70/30 plate are around 380 MPa tensile and 140 MPa yield with elongation in the 40 % region. Annealed material is soft, roughly 35 to 45 HRB. Where a fabricator needs a guaranteed hardness band or a tighter yield window, it should be written into the order rather than assumed, because the grade has a wide natural spread and annealing practice is what moves it.
Behaviour at temperature and at depth
C71500 keeps most of its room-temperature strength to about 300 degrees C, which is why it appears in feedwater heaters and low-pressure steam service as well as in cold seawater. Going the other way, it has no ductile to brittle transition. Impact values hold at liquid nitrogen temperature, so cryogenic and LNG seawater vaporiser duties are within its range. Creep becomes the controlling factor above roughly 350 degrees C.
Physical properties
| Property | Value | Condition |
|---|---|---|
| Density | 8.94 g/cm³ | 20 degrees C |
| Melting range | 1170 to 1240 degrees C | Solidus to liquidus |
| Thermal conductivity | 29 W/m·K | 20 degrees C |
| Coefficient of thermal expansion | 16.2 × 10-6/K | 20 to 300 degrees C |
| Specific heat capacity | 377 J/kg·K | 20 degrees C |
| Electrical resistivity | 375 nΩ·m | 20 degrees C |
| Electrical conductivity | 4.6 % IACS | 20 degrees C |
| Modulus of elasticity | 152 GPa | Tension, annealed |
| Modulus of rigidity | 57 GPa | Torsion, annealed |
| Poisson's ratio | 0.33 | Annealed |
| Relative magnetic permeability | about 1.00 | Annealed, low iron and manganese |
| Machinability rating | 20 | C36000 free-cutting brass = 100 |
Two of these numbers change how the part is designed. The expansion coefficient is roughly 40 % higher than carbon steel, so a C71500 tubesheet bolted or welded into a carbon steel shell carries a differential expansion load that the designer has to account for. And a thermal conductivity of 29 W/m·K is roughly two thirds of the 44 to 46 W/m·K of 90/10 copper-nickel, so a thick 70/30 tubesheet is a real thermal resistance in a way a thin one is not.
C71500 equivalent grades
| System | Designation | Number |
|---|---|---|
| USA, UNS | C71500 | C71500 |
| Europe, EN | CuNi30Mn1Fe | CW354H |
| Germany, DIN | CuNi30Mn1Fe | 2.0882 |
| United Kingdom, BS | CN107 | CZ / CN series |
| Japan, JIS | C7150 | C7150 |
| China, GB | BFe30-1-1 | T71510 |
| France, NF | CuNi30Mn1Fe | U-N30 |
| ISO | CuNi30Mn1Fe | CuNi30Mn1Fe |
| Trade names | Cupronickel 715, Alloy 715, Copper Nickel 70/30 | - |
These are near equivalents, not drop-in substitutes. BFe30-1-1 to GB/T 5231 allows a slightly different manganese and iron window from ASTM B171, and the European CW354H rod and plate standards set their own property minima. Where a drawing quotes one system and the material is bought against another, the difference is worth resolving on paper before the billet is cut.
Seawater performance and service limits
Copper-nickel resists seawater by growing a thin cuprous oxide film. The film takes time to form and it is the film, not the metal, that does the work. Everything that goes wrong with copper-nickel in service is traceable to that film being prevented from forming, stripped off faster than it rebuilds, or poisoned.
| Alloy | Maximum continuous design velocity | Note |
|---|---|---|
| C70600, 90/10 | 3.0 to 3.5 m/s | 3.0 m/s for high reliability systems; BS MA 18 allows 3.5 m/s above 100 mm bore |
| C71500, 70/30 | 3.5 to 4.0 m/s | 3.5 m/s for high reliability systems; 4.0 m/s in general design guidance |
| Either, with entrained sand | Reduce by 1.0 to 1.5 m/s | Sand strips the protective film mechanically |
| Either, minimum flow | 0.5 to 1.0 m/s | Below this, deposits settle and cause local attack |
| Either, bore below 100 mm | Reduced progressively | Local turbulence raises the real velocity at the wall in small bores |
| Either, short duration | 10 to 15 m/s | Transient only, not a design condition |
What causes trouble in practice
- Sulphides. Stagnant or polluted harbour water goes anaerobic and generates sulphide, which produces a black non-protective film in place of the normal one. Exposure during the first weeks of service, before the oxide film has matured, does the most damage.
- Commissioning on the wrong water. Hydrotest and first fill should use clean aerated seawater or fresh water. If a system has been filled with polluted water it should be drained and flushed rather than left standing, and a firefighting line filled with seawater needs the water changed within four or five days.
- Film maturity. A fully developed protective film takes up to three months to establish. Velocity excursions and sulphide exposure in that window matter much more than the same events two years later.
- Galvanic coupling. Copper-nickel is cathodic to carbon steel and anodic to titanium, graphite and most stainless steels in seawater. A 70/30 tubesheet joined to a carbon steel water box will drive corrosion of the steel unless the joint is isolated or sacrificial anodes are sized for it.
- Ammonia. Copper-nickel is far less prone to stress corrosion cracking than brass, but ammonia and amines in condensate systems will still attack it. This is a common reason for specifying 70/30 in the air removal section of a condenser.
Set against that, copper-nickel is immune to chloride stress corrosion cracking, which is the failure mode that rules austenitic stainless steel out of many seawater duties, and it is naturally resistant to macrofouling. Barnacles and mussels do not settle readily on it, so a copper-nickel water box or tubesheet stays clearer than a coated steel one without any biocide dosing.
How C71500 is forged
Copper-nickel forges in a narrower window than steel and punishes carelessness at both ends of it. The working range is 925 to 1025 degrees C. Above that the alloy starts to burn at the grain boundaries; below about 850 degrees C the load climbs steeply and surface cracking follows.
| Operation | Practice |
|---|---|
| Heating | Electric resistance furnaces. Sulphur-free atmosphere, surfaces free of oil, grease and marking compound before charging. |
| Forging range | 925 to 1025 degrees C, finishing above 850 degrees C |
| Reduction | Minimum 3:1 forging ratio from billet, taken in steady passes rather than heavy single bites |
| Reheating | Permitted within the range; the piece is returned to the furnace rather than worked cold |
| Annealing | 650 to 850 degrees C, held by section, then cooled rapidly to keep iron in solution |
| Cooling from forging | Still air on light sections; heavy sections are annealed rather than relied on as-forged |
| Descaling | Pickled or mechanically cleaned; the oxide is tenacious and will otherwise be rolled in |
Sulphur is the one that catches people out. It comes from oil-fired furnace atmosphere, from cutting fluid left on the billet, from crayon marking and from rubber gloves. At forging and annealing temperature it penetrates the grain boundaries and produces intergranular cracking that no amount of subsequent work will close. All heating here is done in electric car-bottom and pit furnaces, which removes the furnace as a source, and the billet is degreased before it is charged.
Heat treatment: what does and does not apply
There is no quench and temper route for this grade and no ageing response. Asking for a normalise achieves nothing. The only heat treatment that changes the material is the anneal, and its purpose is to recrystallise the worked structure, put the iron back into solid solution and remove forging stress. Grain size is reported to ASTM E112 where the order calls for it. Strength above the annealed level is available only by cold work, which is a route for bar and small sections rather than for tubesheets.
Machining and drilling C71500
At a machinability rating of 20, C71500 is gummy. It work-hardens ahead of the tool, produces long stringy chips and conducts heat poorly, so the heat stays in the cutting zone. Tubesheet drilling is the operation where all three show up at once, because a 60 mm thick plate with two thousand holes gives the problem two thousand chances.
- Cut with a positive rake and a sharp edge. Rubbing hardens the surface and the next pass then cuts a harder material.
- Keep feed constant and never let the tool dwell in the cut.
- Flood coolant. Sulphurised cutting oils are avoided here for the reason given above, since traces left on the part become a problem at any later heating or welding operation.
- Use chip breakers and peck cycles for deep holes. Long chips in a tube hole will score the bore, and a scored tube hole is a leak path once the tube is expanded into it.
- Carbide is normal, with high-speed steel workable on light cuts and small holes.
- Expect roughly a third of the metal removal rate of carbon steel, and allow for it in the delivery date rather than in the shop.
Tube holes are drilled to the fabricator's drawing with grooves cut as specified, and hole diameter, ligament and finish are reported against TEMA or the project standard named on the order.
Welding C71500
C71500 welds well. Filler is ERCuNi bare wire to AWS A5.7 for TIG and MIG, and ECuNi covered electrode to AWS A5.6 for manual metal arc. ERCuNi is itself a 70/30 copper-nickel carrying a titanium addition to deoxidise the weld pool, and the same consumable is used on 90/10 base metal as well as on 70/30.
- No preheat. The alloy is single phase and has nothing to preheat for; heat only slows the job and coarsens the grain.
- Keep interpass temperature low, around 150 degrees C or below.
- No post-weld heat treatment is required or wanted.
- Clean back to bright metal before every pass. Copper-nickel weld metal is intolerant of oxide, oil and sulphur, and porosity is almost always traceable to one of them.
- Argon for TIG. Copper-nickel is more fluid than steel, so joint preparations are opened up and root gaps controlled more tightly.
- A 70/30 weld overlay on a carbon steel tubesheet is a common alternative to a solid forging, and we supply both.
For dissimilar joints to carbon steel, the usual practice is to butter the steel side with a 65 % nickel-copper consumable of the ENiCu-7 or ERNiCu-7 type and then weld copper-nickel to the buttering. Direct copper-nickel to carbon steel welds are possible but dilute the copper-nickel enough to compromise its corrosion resistance at the fusion line.
C71500 forgings we produce
Copper-nickel billet is bought from qualified copper mills against the standard named on the order. Forging, annealing, machining and testing are done here, on one site, which is where the lead time and the certification come from.
Tubesheets and tube plates
Fixed, stationary, floating and rear-head tubesheets. Baffles and support plates, drilled and grooved to TEMA or to the fabricator's drawing.
Seamless rolled rings
Ring-rolled blanks for flanges, sleeves, bushings, bearing rings and valve seats, rolled near-net to cut the machining loss on an expensive alloy.
Flanges and valve parts
Weld-neck, blind and plate flanges, pump and valve body blanks, water box components and salt water fittings.
Discs and blanks
Forged discs, blind discs, cover plates and blank rounds for machining into pump and seal components.
Bars and hollow bars
Forged round bar, square and rectangular blocks, hollow bar, propeller sleeves, ferrules and shafts.
Clad and overlaid tubesheets
Carbon steel or low alloy backing with a C71500 weld overlay on the water side, where a solid copper-nickel plate is not economic.
Capability
| Operation | Equipment | Capacity |
|---|---|---|
| Open-die forging | Hydraulic presses, 6,300 t, 4,000 t and 2,000 t | Single pieces to 30 t |
| Ring rolling | Radial-axial mills, 6 m, 3 m and 1 m | OD 50 mm to 6,000 mm |
| Annealing | Electric car-bottom furnaces | Chamber to 8,000 × 2,000 × 2,000 mm |
| Vertical turning | Vertical lathes, 5,000 mm, 3,500 mm and 2,500 mm swing | Discs and tubesheets to 5,000 mm |
| Deep hole drilling | CNC deep-hole machine | 1,600 mm diameter by 10,000 mm |
| Horizontal turning | Horizontal and CNC lathes | To 1,800 mm diameter by 14,000 mm |
Those are the machines, and for copper-nickel they are not the binding constraint. The size of a C71500 forging is limited in practice by the billet a copper mill will supply, so we confirm billet availability before quoting a date rather than after.
Where C71500 forgings are used
| Sector | Components |
|---|---|
| Power generation | Main condenser tubesheets, feedwater heater tubesheets, air removal section components, water box parts |
| Desalination | MSF and MED evaporator tube plates, brine heater tubesheets, distiller components |
| Offshore and marine | Seawater lift pump parts, valve and pump bodies, cooler tubesheets, propeller sleeves, salt water flanges and fittings |
| Naval | Condenser and cooler components, minehunter work where low magnetic permeability is specified |
| Oil, gas and petrochemical | Seawater cooled exchanger tubesheets, brine service components, platform utility systems |
| LNG and cryogenic | Seawater vaporiser components, where the absence of a ductile to brittle transition is the reason for the choice |
Testing, examination and certification
| Test | Method | Scope |
|---|---|---|
| Chemical analysis | Optical emission spectrometry to ASTM E478 | Every heat, reported against the ordered standard |
| Positive material identification | Handheld analyser | On the finished part, on request |
| Tensile | ASTM E8/E8M, general requirements ASTM B248 and B249 | Tensile, yield at 0.5 % extension under load, elongation |
| Hardness | Brinell or Rockwell B | On the part or on the test coupon |
| Grain size | ASTM E112 | On request; usual for tubesheets that will be seal welded |
| Ultrasonic examination | Straight beam contact, to a written procedure agreed on the order | Reference blocks cut from the same alloy and condition, since copper-nickel attenuates differently from steel |
| Liquid penetrant | ASTM E165 | Machined faces and weld overlay surfaces |
| Magnetic permeability | Measured and reported | Where a maximum is stated on the order, as in naval work |
| Dimensional | Against the drawing | Tube hole diameter, ligament, flatness and finish reported for tubesheets |
Magnetic particle examination does not apply to this alloy. Radiography is available through a subcontractor when a weld overlay needs it. Certification is EN 10204 3.1 as standard, and EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or your own inspector when the order calls for it. The works holds CCS, BV, DNV, LR and NK classification society approvals.
How to order C71500 forgings
A price comes back within two working days when the enquiry is complete. Six things make it complete.
- Standard and grade. ASTM B171 C71500, EN CW354H, GB BFe30-1-1 or whatever the drawing quotes. Say if the material is for welding, since that tightens the zinc, lead, phosphorus, sulphur and carbon limits.
- Dimensions or a drawing. PDF, DWG, DXF and STEP are all accepted. For a tubesheet, the hole pattern matters more than the outline.
- Quantity and repeat volume. One-off or four times a year changes how the billet is bought.
- Delivery condition. As-forged, proof machined or finish machined including drilled tube holes.
- Testing. Mechanical test scope, grain size, ultrasonic examination, permeability limit if there is one.
- Certification and destination. EN 10204 3.1 or 3.2, which inspection body, and the port.
Minimum order is 10 kg with no minimum piece count. Lead time runs 20 to 60 days by material route, and copper-nickel sits toward the upper end because the billet is bought in rather than melted here. Nearest ports are Zhangjiagang and Shanghai.
Frequently asked questions about UNS C71500
What is UNS C71500?
A wrought 70/30 copper-nickel containing 29.0 to 33.0 % nickel and 0.40 to 1.0 % iron, with copper as the remainder. It is a single-phase solid solution alloy used for seawater and brine service where flow velocity, impingement or temperature would damage other copper alloys.
Is C71500 the same as CuNi 70/30 and BFe30-1-1?
They describe the same 70/30 cupronickel. C71500, CuNi30Mn1Fe (EN CW354H), DIN 2.0882, BS CN107, JIS C7150 and Chinese BFe30-1-1 all sit in this group. Minor element limits are not identical between standards, so the governing specification has to be named on the purchase order.
What is the difference between C71500 and C70600?
C70600 is 90/10 copper-nickel with about 10 % nickel and 1.0 to 1.8 % iron. C71500 has about 30 % nickel and 0.40 to 1.0 % iron. C71500 is stronger, takes a higher seawater design velocity, and copes better with polluted water. C70600 conducts heat roughly 50 % better, 44 to 46 W/m.K against 29, and costs less, so it stays the usual choice for general seawater piping and condenser tube.
Which standards cover C71500 tubesheets and forgings?
ASTM B171 and ASME SB-171 cover plate, sheet and circles for condensers and heat exchangers, and are the usual route for tubesheets and tube plates. ASTM B151 covers rod and bar, ASTM B122 plate, sheet, strip and rolled bar, ASTM B111 condenser tube, and ASTM B466 and B467 pipe.
What is the maximum seawater velocity for C71500?
Published guidance for 70/30 copper-nickel pipework runs from 3.5 m/s for high reliability systems up to 4.0 m/s, against 3.0 to 3.5 m/s for 90/10. Subtract 1.0 to 1.5 m/s where sand is entrained, and reduce further below 100 mm bore. Local velocity rises at elbows, small bores and tube inlets, so the project design rules take precedence over any single number.
Can C71500 be hardened by heat treatment?
No. C71500 is single phase and has no hardening transformation, so quenching and tempering do nothing for it. Strength above the annealed level comes only from cold work. Heat treatment is limited to annealing between 650 and 850 degrees C to control grain size and relieve forging stress.
Is C71500 magnetic?
Annealed C71500 is close to non-magnetic, with relative permeability near 1.00. Iron and manganese at the top of the range, and heavy cold work, raise it slightly. Minehunter and instrument work should state a maximum permeability on the order so it can be measured and reported.
What filler metal is used to weld C71500?
ERCuNi bare wire to AWS A5.7 for TIG and MIG, and ECuNi covered electrodes to AWS A5.6 for manual metal arc. ERCuNi is a 70/30 copper-nickel with a titanium addition as deoxidiser, and it is used on 90/10 base metal as well. No preheat is used, interpass temperature is kept low, and no post-weld heat treatment is required.
Why does copper-nickel have to be kept away from sulphur during heating?
Sulphur in furnace atmosphere, fuel oil, cutting fluid or marking paint penetrates the grain boundaries of copper-nickel at forging and annealing temperature and causes intergranular cracking. Electric furnaces avoid the problem at source, and surfaces are cleaned of oil, grease and marking compound before any heating operation.
What size C71500 tubesheet can be forged?
The presses run to 6,300 tonnes and the vertical lathes take 5,000 mm swing, so disc and tubesheet blanks are handled well beyond the size of most copper-nickel exchangers. The practical limit on any given job is the billet the copper mill can supply, which is confirmed at enquiry stage before a delivery date is given.
Can you supply a carbon steel tubesheet with a C71500 overlay instead?
Yes, and on large exchangers it is often the cheaper answer. The backing plate carries the pressure and the overlay carries the corrosion duty. Overlay thickness after machining is normally 5 to 8 mm, and the finished surface is penetrant tested.
Does C71500 suffer chloride stress corrosion cracking?
No. That is one of the main reasons it is specified in place of austenitic stainless steel in seawater. It is, however, attacked by ammonia and amines, which is a separate consideration in condensate and air removal systems.
About the manufacturer
Jiangyin Jiangnan Metal has been forging since 1997 at Zhouzhuang Town, Jiangyin, on the south bank of the Yangtze between Shanghai and Nanjing. The site runs a melt shop, three open-die presses, three ring mills, fourteen heat treatment furnaces, a machine shop and a laboratory, with 460 people including 9 senior and 32 intermediate engineers.
For steel and nickel alloys the metal is melted here. For copper-nickel it is not: billet is bought from qualified copper mills, and what we add is the forging, the annealing, the machining and the testing. Technical questions about this grade are answered by an engineer on site rather than passed along. Enquiries are handled in English and Chinese, Monday to Saturday, 08:00 to 17:30 China Standard Time.
Related grades on this site: Monel 400 for higher strength seawater service, Inconel 625 where copper-nickel runs out of velocity or temperature headroom, and duplex stainless steels where chloride cracking risk is manageable. See also forged tube sheets and seamless rolled rings.
Need a price for a C71500 forging?
Send the drawing and the standard. A quotation comes back within two working days, and an engineer rather than a sales clerk answers the technical part of it.
Send an enquiry +86 189 2135 9659
Phone, WhatsApp and WeChat use the same number. Plant address: No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China 214423.