What SNCM431 is
SNCM431 is one of the 40 low-alloy structural steels listed in JIS G4053, Japan's standard for hot-rolled, hot-forged and hot-extruded machine structural steel. The prefix reads directly: Steel, Nickel, Chromium, Molybdenum. Under the older JIS G4103 numbering the same grade was designated SNCM 1.
Nickel at 1.60 to 2.00 % is what separates SNCM431 from the Cr-Mo grades such as SCM435 and SCM440. Nickel raises hardenability and, more importantly, keeps toughness from collapsing as strength rises. It is the only common alloying element that improves low-temperature impact properties. Molybdenum at 0.15 to 0.30 % suppresses temper embrittlement, so the steel can be tempered in the 580 to 680 °C range without losing toughness on slow cooling through the critical band. Together they make Ni-Cr-Mo steel the usual choice for large sections that have to be tough right through rather than only at the surface.
SNCM431 is a through-hardening grade, not a case-hardening grade. Its carbon content is high enough that quenching and tempering develop strength in the bulk of the section. This distinguishes it from the carburising members of the same family, SNCM220, SNCM415, SNCM420, SNCM616 and SNCM815, which carry 0.12 to 0.23 % C and are case-hardened after machining. Datasheets that quote a double quench of 850 to 900 °C followed by 780 to 830 °C and a 150 to 200 °C temper for SNCM431 have copied the carburising schedule from SNCM420 by mistake; that is not the correct treatment for this grade.
- Designation
- SNCM431 (JIS G4053); formerly SNCM 1 under JIS G4103
- Family
- Nickel-chromium-molybdenum structural steel, through-hardening
- Standard
- JIS G4053:2016 (reissued 2018), covering bars, wire rod, plate, strip, flats, hot-forged and hot-extruded sections
- Condition supplied
- As-forged, normalised, annealed, or quenched and tempered to an agreed property band
- Typical hardness, Q&T
- 248 to 302 HB (approx. 24 to 32 HRC)
- Nearest US grades
- AISI / SAE 4330 or 4337, not 4340
- Forged here as
- Seamless rolled rings, forged rings, shafts, bars, blocks, discs, hollow cylinders
- Size envelope
- 10 kg to 30,000 kg single piece; rings to OD 6,000 mm; shafts to 14,000 mm turned length
- Certification
- EN 10204 3.1 standard; 3.2 witnessed by BV, DNV, LR, SGS, TÜV or the customer on request
- Producer
- Jiangyin Jiangnan Metal Co., Ltd., Zhouzhuang Town, Jiangyin, Jiangsu, China
Chemical composition
The figures below are the ladle-analysis limits given in Table 2 of JIS G4053:2016. They are the only properties the current edition of the standard actually specifies for this grade.
| Element | C | Si | Mn | P | S | Ni | Cr | Mo | Cu |
|---|---|---|---|---|---|---|---|---|---|
| Specified % | 0.27–0.35 | 0.15–0.35 | 0.60–0.90 | ≤ 0.030 | ≤ 0.030 | 1.60–2.00 | 0.60–1.00 | 0.15–0.30 | ≤ 0.30 |
| Role | Strength, hardenability | Deoxidation | Hardenability, S control | Impurity | Impurity | Toughness, hardenability | Hardenability, temper resistance | Suppresses temper embrittlement | Residual limit |
Balance iron. Elements not listed in the table must not be added intentionally other than to finish the steel. Copper is a residual limit, not an alloying addition. Where product analysis is agreed instead of ladle analysis, the permissible variations of JIS G0321 Table 4 apply.
SNCM431 is melted in a 25 t electric arc furnace and refined in a 25 t or 50 t ladle furnace, with vacuum oxygen decarburisation available where tighter gas or sulphur control is specified. Because the steel is melted on site rather than bought in as billet, the aim analysis can be set for the forging it will become, for example biasing carbon toward the upper half of the range for a heavy section that must still reach hardness at mid-radius.
Mechanical properties after quenching and tempering
The current edition of JIS G4053 does not specify mechanical properties. The standard deliberately limits itself to chemical composition, appearance, shape, dimensions and tolerances, on the stated reasoning that properties after quenching and tempering depend heavily on the user's equipment and heat-treatment practice, so fixing values in the standard would mislead rather than help. The figures below are the long-established reference values carried in JIS G4103 and reproduced in the JIS handbooks and Japanese design tables. Treat them as the benchmark a 25 mm test piece should meet, then agree the actual acceptance values for your section size in the purchase order.
| Property | Metric | Imperial |
|---|---|---|
| Yield point / 0.2 % proof stress | ≥ 685 N/mm² (685 MPa) | ≥ 99 ksi |
| Tensile strength | ≥ 830 N/mm² (830 MPa) | ≥ 120 ksi |
| Elongation, A | ≥ 20 % | ≥ 20 % |
| Reduction of area, Z | ≥ 55 % | ≥ 55 % |
| Charpy impact value (U-notch) | ≥ 98 J/cm² | ≥ 47 ft·lbf/in² |
| Hardness | 248–302 HB | approx. 24–32 HRC |
Reference values for the quenched-and-tempered condition on a standard test piece. Properties in a heavy forged section fall below test-piece values as ruling section increases, because the cooling rate at mid-radius is slower than at the test piece. For sections over roughly 150 mm, state the location and depth at which properties must be met.
Practical tempering response
Tempering temperature is the control the buyer actually has. Within the 580 to 680 °C range the same steel can be delivered anywhere from roughly 300 HB down to 250 HB, trading strength against toughness and machinability.
| Tempering temperature | Indicative hardness | Character |
|---|---|---|
| 580–600 °C | approx. 290–320 HB | Upper end of the strength band; used where fatigue strength governs and machining is light |
| 600–640 °C | approx. 265–295 HB | The usual delivery band for shafts, gear blanks and rings; balanced strength and toughness |
| 640–680 °C | approx. 240–275 HB | Maximum toughness and best machinability; chosen for thick sections and low-temperature service |
Indicative values from this works' heat-treatment practice, not standard requirements. Actual results depend on section size, quench severity and soak time, and are confirmed on a representative test piece heat-treated with the forging.
Ni-Cr steels are susceptible to reversible temper embrittlement if cooled slowly through roughly 600 to 450 °C after tempering. The molybdenum in SNCM431 largely suppresses it, and this works also quenches from the tempering temperature in oil or water rather than cooling in the furnace. For sour service or low-temperature duty, specify a step-cool embrittlement test on the enquiry so it is scheduled before shipment.
Heat treatment
| Operation | Temperature | Cooling | Purpose |
|---|---|---|---|
| Forging | 1,150–1,200 °C start ≥ 850 °C finish | Air, then controlled cool | Work the ingot; close porosity; develop grain flow |
| Normalising | 850–880 °C | Air | Refine as-forged grain, homogenise before hardening |
| Annealing (softening) | 810–850 °C | Furnace cool to approx. 550 °C, then air | Soften to approx. 220 HB for rough machining |
| Stress relief | 550–650 °C | Furnace cool | Relieve machining and straightening stresses below the tempering temperature |
| Hardening (quench) | 820–870 °C | Oil | Transform to martensite through the section |
| Tempering | 580–680 °C | Rapid, oil or water | Set final strength and toughness; rapid cool avoids temper embrittlement |
Quenching and tempering temperatures follow the JIS reference schedule for SNCM431. Forging, normalising, annealing and stress-relief ranges are this works' practice for the grade. Soak times scale with section thickness; the usual rule of one hour per 25 mm of ruling section is a starting point, not a substitute for a furnace chart.
Why section size matters more than the schedule
SNCM431 has good hardenability: the nickel and molybdenum let it harden through sections that would leave a plain carbon steel soft at the core. That does not make it unlimited. Beyond roughly 150 to 200 mm ruling section, the quench cannot cool mid-radius fast enough for full martensite, and strength at the centre falls below the test-piece figures. Two things follow for anyone buying a heavy SNCM431 forging. First, specify where the test piece is taken from (surface, mid-radius or centre), because the same forging will give different answers. Second, if properties have to hold at the centre of a very heavy section, SNCM439 or a higher-alloy grade may be the right specification rather than a tighter heat treatment on SNCM431.
Fourteen furnaces, all in-house. Car-bottom furnaces take work up to 8,000 × 2,000 × 2,000 mm for rings, discs and blocks. Two well-type furnaces 15 m deep by Ø1,500 mm let long SNCM431 shafts be quenched vertically, which controls the distortion that horizontal quenching produces on a slender shaft. Every cycle is recorded and the chart is issued with the certificate.
Physical properties
JIS G4053 specifies no physical properties. The values below are typical of quenched-and-tempered low-alloy Ni-Cr-Mo steel at 20 °C and are given for design calculation, not as acceptance criteria.
| Property | Typical value | Unit |
|---|---|---|
| Density | 7.85 | g/cm³ (kg/dm³) |
| Modulus of elasticity | 205 | GPa |
| Shear modulus | 80 | GPa |
| Poisson's ratio | 0.29 | – |
| Thermal conductivity | approx. 42 | W/(m·K) |
| Specific heat capacity | approx. 460 | J/(kg·K) |
| Mean coefficient of thermal expansion, 20–100 °C | approx. 11.5 × 10⁻⁶ | 1/K |
| Mean coefficient of thermal expansion, 20–300 °C | approx. 12.7 × 10⁻⁶ | 1/K |
| Electrical resistivity | approx. 0.22 | µΩ·m (22 µΩ·cm) |
| Melting range | approx. 1,420–1,460 | °C |
Typical values for the grade family, not specification minima. Thermal conductivity falls and specific heat rises with temperature; use temperature-dependent data for thermal-stress work.
Equivalent and near-equivalent grades
A large number of published cross-reference tables list SNCM431 against AISI 4340, DIN 34CrNiMo6 / 1.6582 and BS 817M40. That row belongs to SNCM439. SNCM439 carries 0.36 to 0.43 % C, which matches 4340's 0.38 to 0.43 %. SNCM431 carries 0.27 to 0.35 % C and sits one full strength class lower, at 830 MPa minimum tensile against 980 MPa. Ordering 4340 when the drawing calls for SNCM431 will pass a chemistry check on nickel, chromium and molybdenum and fail it on carbon.
| Standard | Designation | Closeness | Note |
|---|---|---|---|
| JIS G4053 (Japan) | SNCM431 | Identical | The grade itself |
| JIS G4103 (superseded) | SNCM 1 | Identical | Former Japanese designation for the same steel |
| AISI / SAE (USA) | 4330 | Close | 0.28–0.33 C, 1.65–2.00 Ni, 0.70–0.90 Cr, 0.20–0.30 Mo; nearest match on carbon |
| AISI / SAE (USA) | 4337 | Close | 0.35–0.40 C, at the top of the SNCM431 carbon range |
| EN 10083-3 (Europe) | 36CrNiMo4 / 1.6511 | Approximate | Same strength class; nickel lower at 0.90 to 1.20 % |
| EN 10083-3 (Europe) | 34CrNiMo6 / 1.6582 | Not equivalent | Cr 1.30 to 1.70 %; maps to SNCM439 |
| BS 970 (UK) | 816M40 / 817M40 | Not equivalent | 4340 class; maps to SNCM439 |
| GB/T 3077 (China) | No exact grade | Approximate | Nearest by composition is the 30Cr–2Ni–Mo family; 40CrNiMoA corresponds to SNCM439, not SNCM431 |
Cross-references compare nominal chemistry and strength class. They are a starting point for substitution, never an authorisation. Where a drawing or code names SNCM431, confirm substitution in writing with the design authority before the steel is melted.
SNCM431 against the grades it is usually confused with
| Property | SNCM431 | SNCM439 | SCM440 |
|---|---|---|---|
| Carbon % | 0.27–0.35 | 0.36–0.43 | 0.38–0.43 |
| Nickel % | 1.60–2.00 | 1.60–2.00 | ≤ 0.25 |
| Chromium % | 0.60–1.00 | 0.60–1.00 | 0.90–1.20 |
| Molybdenum % | 0.15–0.30 | 0.15–0.30 | 0.15–0.30 |
| Yield, reference | ≥ 685 MPa | ≥ 885 MPa | ≥ 835 MPa |
| Tensile, reference | ≥ 830 MPa | ≥ 980 MPa | ≥ 980 MPa |
| Nearest US grade | 4330 / 4337 | 4340 | 4140 / 4142 |
| Choose it when | Toughness and a forgiving heat treatment matter more than peak strength | Peak strength is needed in a heavy section | Nickel is not required and cost matters |
Reference strength values for the quenched-and-tempered condition on a standard test piece. All three grades are forged and heat-treated at this works.
Where SNCM431 is used
SNCM431 is specified where a part must carry high cyclic load through a substantial section and stay tough. It is the grade you move to when SCM440 lacks the hardenability or the impact properties, and SNCM439 is more strength than the design needs.
Power transmission
Gear shafts, pinion shafts, spindles, gear wheels, ring gears and gearbox output shafts, where bending fatigue and tooth-root stress govern.
Forged as: shafts, gear blanks, ring gear preforms
Heavy machinery
Eccentric shafts, press components, rolls, crane wheels, connecting rods and drive couplings running under repeated shock load.
Forged as: shafts, discs, hollow forgings
Marine and propulsion
Propeller shaft sections, rudder stocks, couplings and stern-tube components, where the nickel content carries impact properties into cold water service.
CCS, BV, DNV, LR and NK approved works
Bearings and slewing rings
Seamless rolled rings for bearing races, slewing rings, yaw and pitch rings, and gear ring blanks rolled to contoured section.
Ring OD 50 mm to 6,000 mm
Fasteners and highly stressed bolting
Studs, tie rods, anchor bolts and large-diameter bolting for flanged joints and structural connections.
Forged as: bars, upset blanks
Tooling and die holders
Die blocks, bolsters, mould frames and holders that need toughness under impact rather than wear resistance at the surface.
Forged as: blocks, plates, slabs
SNCM431 forged product forms and size envelope
Every form below is forged from a single piece of steel melted on this site: no welding, no casting, no purchased billet of unknown origin. Each size limit is set by a specific machine, named alongside it.
| Form | Description | Size limit | Set by |
|---|---|---|---|
| Seamless rolled rings | Rectangular and contoured section; bearing races, slewing rings, gear ring blanks | OD 50 to 6,000 mm | 6 m radial-axial ring mill; 3 m and 1 m mills for smaller sizes |
| Forged rings | Upset and punched rings outside the ring-mill envelope, or needing heavy reduction | to 30,000 kg | 6,300 t hydraulic press |
| Gear shafts, pinion shafts, spindles | Stepped, eccentric and flanged shafts; rotors; tie rods | to 14,000 mm turned length | C61160 horizontal lathe; 15 m well furnace for vertical quench |
| Round, square, flat and hex bars | Forged bar stock for machined parts, fasteners and tooling | to 30,000 kg per piece | 6,300 t, 4,000 t and 2,000 t presses; 5 t to 750 kg hammers |
| Blocks, discs, plates, tube sheets | Solid forged discs and die blocks, proof-machined for volumetric inspection | to Ø5,000 mm machined | Ø5,000 mm vertical turning lathe |
| Hollow bars, sleeves, bushings, cylinders | Bored from solid forged blanks: sleeves, bushes, barrels, casings, housings, hubs | to Ø1,600 × 10,000 mm bore | CNC deep-hole drilling machine |
Minimum order 10 kg, with no minimum piece count, so a single one-off part is quotable. Very small parts are grouped into a batch to share furnace and setup time, which is why quantity still affects unit price.
Delivery condition
- As-forged with machining allowance, normalised or annealed for the customer's own heat treatment
- Quenched and tempered to an agreed hardness or property band, with the furnace chart issued
- Proof-machined to a surface suitable for ultrasonic examination to ASTM A388 or EN 10228-3
- Finish-machined to drawing, including bored, stepped and flanged features
Testing, certification and traceability
Because SNCM431 is melted here, chemistry is verified at the furnace rather than taken from a supplier's certificate. The traceability chain runs from melt number through forging, heat treatment and machining to shipment, instead of starting at a purchased billet.
| Test | Method | Standard |
|---|---|---|
| Chemical analysis | Optical emission spectrometry at the furnace and on the product | ASTM E415 |
| Carbon and sulphur | Infrared combustion analyser | ASTM E1019 |
| Alloy verification | Handheld PMI analyser on the finished part | Positive material identification |
| Tensile | 600 kN and 300 kN universal testing machines | ASTM A370, ISO 6892 |
| Impact | Pendulum impact tester with low-temperature bath, to −60 °C | ASTM A370 |
| Hardness | Leeb hardness tester, converted | ASTM A956, ASTM E140 |
| Ultrasonic examination | Full-digital flaw detectors on proof-machined surfaces | ASTM A388, EN 10228-3 |
| Magnetic particle | Multipurpose MPI crack detection | ASTM E709 |
| Grain size and microstructure | Metallographic preparation and microscopy | ASTM E112 |
Tests outside this scope, for example impact testing below −60 °C or bench Brinell where a portable instrument is not accepted, are placed with an accredited third-party laboratory and reported alongside the mill certificate. State the requirement at enquiry stage so it is scheduled before shipment.
Certification
- EN 10204 3.1 mill test certificate as standard on every SNCM431 order
- EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TÜV or the customer's own inspector, on request
- Class approvals held: CCS, BV, DNV, LR and NK
- Supporting records: heat-treatment charts, NDT reports, dimensional reports, PMI records
How to order SNCM431 forgings
Quotations are prepared from a drawing or a written specification. Sending the six items below in the first email removes a round trip and usually gets a price back within two working days.
| No. | Item | Example |
|---|---|---|
| 1 | Grade and standard | SNCM431 to JIS G4053 |
| 2 | Form and dimensions, or a drawing (PDF, DWG, DXF, STEP) | Seamless rolled ring, OD 1,200 × ID 900 × H 260 mm |
| 3 | Quantity and expected repeat volume | 12 pcs, about 4 times per year |
| 4 | Delivery condition | Quenched and tempered, 262 to 302 HB, proof-machined |
| 5 | Testing requirements and where properties must be met | Tensile and Charpy at mid-radius; UT to ASTM A388 |
| 6 | Certification and destination port | EN 10204 3.2 witnessed by DNV, Rotterdam |
- Minimum order
- 10 kg, no minimum piece count
- Typical lead time
- 20 to 35 days from order confirmation. SNCM431 takes the electric-arc and ladle-furnace route with no remelting step, so it sits at the lower end of the works' 20 to 60 day band
- Quotation turnaround
- Normally within two working days of a complete enquiry
- Export experience
- North America, Europe, the Middle East and Asia-Pacific, since 1997
- Audits and inspection
- Customer audits, pre-shipment inspection and third-party witness testing welcome; arrange by email so an English-speaking engineer is available
Frequently asked questions about SNCM431
What is SNCM431 steel?
SNCM431 is a nickel-chromium-molybdenum structural steel specified in JIS G4053, the Japanese standard for low-alloy machine structural steel. It contains 0.27 to 0.35 % carbon, 1.60 to 2.00 % nickel, 0.60 to 1.00 % chromium and 0.15 to 0.30 % molybdenum, with phosphorus and sulphur each limited to 0.030 % and copper to 0.30 %. It is a through-hardening grade used for shafts, gears, rings and other highly stressed machine components, and was designated SNCM 1 under the superseded JIS G4103. Jiangyin Jiangnan Metal Co., Ltd. melts and forges SNCM431 in Jiangyin, Jiangsu Province, China.
What are the mechanical properties of SNCM431?
In the quenched-and-tempered condition on a standard test piece, SNCM431 reaches a yield point of at least 685 MPa, a tensile strength of at least 830 MPa, elongation of at least 20 %, reduction of area of at least 55 %, a Charpy impact value of at least 98 J/cm² and a hardness of 248 to 302 HB. The current edition of JIS G4053 does not itself specify mechanical properties. It covers chemical composition, dimensions and tolerances only, because properties after heat treatment depend on the user's equipment and practice. These figures are the long-standing reference values from JIS G4103 and the JIS handbooks, and should be confirmed as contractual acceptance values for your section size.
Is SNCM431 the same as AISI 4340?
No. AISI 4340 corresponds to SNCM439, not SNCM431. The two Japanese grades share identical nickel, chromium and molybdenum ranges but differ in carbon: SNCM431 carries 0.27 to 0.35 % and SNCM439 carries 0.36 to 0.43 %, matching 4340's 0.38 to 0.43 %. That difference puts SNCM439 a full strength class above SNCM431, at 980 MPa minimum tensile against 830 MPa. Many cross-reference tables repeat the SNCM431 = 4340 = 34CrNiMo6 = 817M40 row in error. By composition the nearest American grades to SNCM431 are AISI/SAE 4330 and 4337.
What is the heat treatment for SNCM431?
Harden by quenching from 820 to 870 °C in oil, then temper at 580 to 680 °C with rapid cooling in oil or water. The rapid cool after tempering matters: nickel-chromium steels are susceptible to reversible temper embrittlement if cooled slowly through roughly 600 to 450 °C, and although the molybdenum content largely suppresses it, quenching from the tempering temperature removes the risk. For softening before machining, anneal at 810 to 850 °C and furnace-cool to about 550 °C. Schedules that call for a double quench and a 150 to 200 °C temper have been copied from the carburising grades SNCM420 or SNCM220 and do not apply to SNCM431.
Can SNCM431 be welded?
It can be welded, but it is not a weld-fabrication steel. At 0.27 to 0.35 % carbon with nickel, chromium and molybdenum, the carbon equivalent is high enough that the heat-affected zone will harden and is susceptible to hydrogen cracking. Welding requires preheat, low-hydrogen consumables, controlled interpass temperature and post-weld heat treatment, and any weld in a quenched-and-tempered part will locally alter the properties the heat treatment established. For load-bearing SNCM431 components this works does not weld; every forging is produced from a single piece of steel.
How large a section can be hardened through in SNCM431?
SNCM431 has good hardenability thanks to its nickel and molybdenum content, but that does not make it unlimited. Beyond roughly 150 to 200 mm ruling section the quench cannot cool the mid-radius fast enough for full martensite, and strength at the centre falls below test-piece values. Two things follow when buying a heavy SNCM431 forging: specify where the test piece is taken from, because surface, mid-radius and centre will give different answers, and consider SNCM439 or a higher-alloy grade if properties have to hold at the centre of a very heavy section.
What forms can SNCM431 be supplied in, and in what sizes?
Jiangyin Jiangnan Metal supplies SNCM431 as seamless rolled rings from OD 50 mm to OD 6,000 mm, forged rings, gear and pinion shafts to 14,000 mm turned length, round, square, flat and hex bars, blocks, discs, plates and tube sheets to Ø5,000 mm machined, and hollow bars, sleeves, bushings and cylinders bored to Ø1,600 × 10,000 mm. The heaviest single piece is 30 tonnes, set by the 60 t maximum heat size and the 6,300 t press. Minimum order is 10 kg with no minimum piece count.
What is the lead time and minimum order for SNCM431 forgings?
Minimum order is 10 kg, with no minimum piece count, so a single one-off part is quotable. Typical lead time is 20 to 35 days from order confirmation. SNCM431 is melted in the electric arc furnace and refined in a ladle furnace without an intermediate vacuum arc or electroslag remelting step, which places it at the lower end of the works' overall 20 to 60 day band. Witnessed third-party inspection to EN 10204 3.2 or testing placed with an outside laboratory needs scheduling, so flag both at enquiry stage.
Does Jiangyin Jiangnan Metal melt its own SNCM431, or buy billet?
It melts its own. SNCM431 is produced in a 25 t electric arc furnace, refined in 25 t and 50 t ladle furnaces with vacuum oxygen decarburisation available, then forged, heat-treated, machined and tested without leaving the site. Maximum heat size is 60 tonnes. This matters on two counts. The aim chemistry can be set for the forging the steel will become rather than accepted as delivered, and the certificate traces the part back to its melt number instead of stopping at a purchased billet certificate.
Which certification is issued with SNCM431 forgings?
An EN 10204 3.1 mill test certificate is issued as standard, covering melt analysis, mechanical test results, heat-treatment records and non-destructive examination. EN 10204 3.2 certification witnessed by Bureau Veritas, DNV, Lloyd's Register, SGS, TÜV or the customer's own inspector is available on request. The works holds CCS, BV, DNV, LR and NK classification society approvals.
Sources and how to cite this page
Standards and references used
- JIS G4053:2016 (reissued 2018), Low-alloyed steels for machine structural use. Table 1 grade designations and Table 2 chemical composition. Annex JC records that mechanical properties after heat treatment are deliberately not specified.
- JIS G4103 (superseded), Nickel chromium molybdenum steels. Reference heat-treatment schedule and property values, retained in the JIS handbooks and Japanese design tables.
- JIS G0320 and JIS G0321, ladle and product analysis methods and permissible variations.
- EN 10204, inspection document types 3.1 and 3.2.
- Heat-treatment practice, size envelope, commercial terms and test scope: works records of Jiangyin Jiangnan Metal Co., Ltd.
Cite this page
Jiangyin Jiangnan Metal Co., Ltd. (2026). SNCM431 Forgings: JIS G4053 Ni-Cr-Mo Steel. Retrieved from https://www.steelforgepieces.com/Alloy-Steel/SNCM431.html
Published by Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Last updated .
Reference property values on this page are given for engineering guidance. They are not a warranty and they are not a substitute for the governing specification or for values agreed in a purchase order. Where a figure on another site conflicts with one here, check it against JIS G4053 and the JIS handbook before designing to it. The widely republished 226 MPa yield and 485 MPa tensile figures for SNCM431 belong to a different material. Corrections are welcome at sales@steelforgepieces.com.