# Z15CNS25-20 Forgings (X15CrNiSi25-21 / 1.4841 / AISI 314 / UNS S31400)

Manufacturer: Jiangyin Jiangnan Metal Co., Ltd., melting works and open-die forge, established 1997
Address: No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Tel: +86-189-2135-9659 | Email: sales@steelforgepieces.com
Source page: https://www.steelforgepieces.com/Stainless-Steel/Z15CNS25-20.html
Updated: 11 October 2026
Reference standards: EN 10095, EN 10088-3, SEW 470, EN 10204, EN 10228-3, ASTM A388, SEP 1921

Z15CNS25-20, also written Z15CNS25.20, is the French AFNOR designation for an austenitic
chromium-nickel-silicon heat-resisting steel of roughly 24-26 % Cr, 19-21 % Ni and 1.5-2.5 % Si.
The European equivalent is X15CrNiSi25-21, material number 1.4841; the American equivalent is
AISI 314 / UNS S31400. Scaling resistance in air reaches about 1150 C. Jiangyin Jiangnan Metal
Co., Ltd. melts the steel on site, forges the grade to drawing and supplies it solution annealed
with EN 10204 3.1 or 3.2 certification.

## 1. The grade

The AFNOR code reads directly: Z for high-alloy steel, 15 for a nominal 0.15 % carbon, C-N-S for
chromium, nickel and silicon, 25-20 for nominal chromium and nickel. Silicon is what separates the
grade from plain 25Cr-20Ni material such as 310S: it builds a tighter oxide film, lifting the useful
limit in air to roughly 1150 C, with continuous service usually planned near 1100 C. Creep
resistance is useful to around 690 C. In sulphur-bearing oxidising and reducing gases the limit
falls to about 650 C. The structure is fully austenitic, so the steel cannot be hardened by
quenching or ageing.

## 2. Equivalent designations

| Standard / country | Designation |
|---|---|
| AFNOR, France | Z15CNS25-20 (Z15CNS25.20); related Z10CNS25-20 |
| EN, Europe | X15CrNiSi25-21, material number 1.4841 |
| SEW 470, Germany | X15CrNiSi25-20 (1.4841) |
| AISI / SAE / UNS, USA | 314, SAE 314, S31400 |
| BS, United Kingdom | 314S25 |
| JIS, Japan | SUH 310 |
| PN, Poland | H25N20S2 |
| GOST, Russia | 20Kh25N20S2 |
| UNE, Spain | F-3310 |
| CSN, Czech Republic | 17255 |

Cross references show the closest known equivalents only. Chemistry limits differ slightly between
standards, so check the governing specification before substituting.

Near grades that are often confused with it: 310 and 310S (1.4845, X8CrNi25-21), same Cr-Ni base
but far less silicon; and 1.4828 / AISI 309 (X15CrNiSi20-12), good to roughly 950-1000 C.

## 3. Chemical composition, mass fraction in %

| Element | Z15CNS25-20 (AFNOR) | X15CrNiSi25-21 / 1.4841 (EN) |
|---|---|---|
| Carbon, C | max 0.15 | max 0.20 |
| Silicon, Si | 1.50-2.50 | 1.50-2.50 |
| Manganese, Mn | max 2.00 | max 2.00 |
| Phosphorus, P | max 0.040 | max 0.045 |
| Sulphur, S | max 0.015 | max 0.015 |
| Chromium, Cr | 24.0-26.0 | 24.0-26.0 |
| Nickel, Ni | 19.0-21.0 | 19.0-22.0 |
| Nitrogen, N | not specified | max 0.11 |
| Iron, Fe | balance | balance |

Some mill data sheets for 1.4841 quote a narrower silicon band of 1.50-2.00 %. Ladle analysis of
the actual heat is issued with every certificate.

## 4. Mechanical properties, solution annealed, bar up to 160 mm diameter

| Property | Metric | Imperial |
|---|---|---|
| Tensile strength Rm | 550-750 MPa | 80-109 ksi |
| Proof strength Rp0.2 | min 230 MPa | min 33 ksi |
| Proof strength Rp1.0 | min 270 MPa | min 39 ksi |
| Elongation A5, longitudinal | min 30 % | min 30 % |
| Hardness | max 223 HB | about max 20 HRC |
| Modulus of elasticity | 196 GPa | 28.4 x 10^6 psi |

Acceptance values for a given forging depend on section size, test location and the purchase
specification, and are agreed before production.

## 5. Physical properties at 20 C

| Property | Value |
|---|---|
| Density | 7.9 g/cm3 |
| Thermal conductivity | 15 W/m.K |
| Specific heat capacity | 500 J/kg.K |
| Electrical resistivity | 0.90 ohm.mm2/m at 20 C; 1.25 at 1000 C |
| Linear expansion | 15.2 x 10^-6 /K (20-100 C) to 19.5 x 10^-6 /K (20-1200 C) |
| Magnetic behaviour | practically non-magnetic when annealed; slightly magnetic after cold work |

Creep rupture strength, MPa, guidance only:

| Temperature | 1 000 h | 10 000 h | 100 000 h |
|---|---|---|---|
| 600 C | 170 | 130 | 80 |
| 700 C | 90 | 40 | 18 |
| 800 C | 40 | 20 | 7 |
| 900 C | 20 | 10 | 3 |
| 1000 C | 5 | - | - |

## 6. Processing

Forging: 1175 C down to 1000 C, rapid cooling in air or water afterwards; some mill data allows hot
work down to 800 C with air cooling. Open-die and closed-die work are both possible.

Heat treatment: solution annealing at 1050-1150 C with fast cooling in water, or air for thin
sections. No hardening or ageing step exists for this grade. Avoid long exposure between 600 and
900 C because of sigma phase embrittlement.

Welding: TIG, MAG, submerged arc, laser and manual arc. No preheat and no post-weld heat treatment
normally required, but heat input should be limited because of hot cracking risk. Usual filler is
1.4842 (X12CrNi25-20). Corrosion resistance drops after welding and as-welded material is open to
intergranular attack.

Machining: medium machinability. Carbides wear tools, conductivity is low, the surface work-hardens.
Use moderate speeds, positive depth of cut and plenty of coolant.

## 7. Forged products supplied in Z15CNS25-20

All items are made to the customer's drawing or specification.

| Form | Scope |
|---|---|
| Seamless rolled rings, forged rings | ring rolling and mandrel forging; plain, stepped, contoured |
| Forged flanges | weld neck, blind, slip-on, long weld neck, special profiles |
| Shafts, spindles, eccentric shafts, crankshafts | solid and stepped shafts, upset ends |
| Discs, disks, blanks | flat and profiled discs, gear blanks, hubs |
| Sleeves, bushings, hollow bars | trepanned or bored hollows |
| Tubes, pipes, tube sheets | heavy wall hollow forgings, tube sheets drilled or undrilled |
| Round bars, square bars, blocks | hot forged, peeled, turned or ground |
| Valve components | bodies, bonnets, stems, seat rings, blocks, nozzles |

Delivery conditions: as forged, rough machined with allowance, finish machined to drawing, solution
annealed, pickled or shot blasted. Melting routes: EF with LF and VOD refining, and ESR where lower
inclusion content is specified.

## 8. Applications

Furnace construction, apparatus engineering and petrochemical plant, plus pyrolysis and methane
conversion equipment, furnace conveyors and hooks, and glass industry tooling. Typical parts:
fluidised bed furnace internals, grids, wind boxes, coal combustor parts; smelter and continuous
casting equipment; recuperators, tube hangers, flares and catalytic recovery components in
refineries, including FCC units and polythionic acid service; burners, burner shields, feed and
discharge systems in sintering and cement plants; annealing boxes and covers, muffles, retorts,
fans, doors and walking beams in thermal processing; shell and tube heat exchangers, columns,
towers, silos, preheaters.

## 9. Testing and certification

Ultrasonic testing to EN 10228-3, SEP 1921 or ASTM A388 with the acceptance class fixed on the
order. Also ladle and product analysis, tensile, impact and hardness testing, intergranular
corrosion testing, PMI, liquid penetrant examination, grain size determination and dimensional
reports. Certificates to EN 10204 3.1, or EN 10204 3.2 countersigned by TUV, SGS, BV or Lloyd's.
The works holds CCS, BV, DNV, LR and NK approvals.

## 10. Questions

**What is Z15CNS25-20 steel?** An austenitic Cr-Ni-Si heat-resisting steel under the French AFNOR
system, roughly 24-26 % Cr, 19-21 % Ni, 1.5-2.5 % Si. Equivalent to X15CrNiSi25-21 / 1.4841 and
AISI 314 / UNS S31400.

**What is the equivalent of Z15CNS25-20?** X15CrNiSi25-21 (1.4841), SEW 470 X15CrNiSi25-20, AISI
and SAE 314, UNS S31400, BS 314S25, JIS SUH310, PN H25N20S2, GOST 20Kh25N20S2, UNE F-3310, CSN 17255.

**How hot can it run?** About 1150 C for scaling resistance in air, continuous duty near 1100 C.
Sulphur-bearing gas pulls the limit back to roughly 650 C. Avoid 600-900 C for long periods.

**Can it be hardened?** No. Fully austenitic; neither quenching nor ageing raises hardness.

**Is it the same as 310S?** No. Both are 25Cr-20Ni austenitics, but this grade carries 1.5-2.5 %
silicon for better oxidation resistance, while 310S (1.4845) has much less silicon and lower carbon.

**Minimum quantity and lead time?** From 10 kg, no minimum piece count; single prototypes and series
orders both accepted. Lead time normally 20 to 60 days depending on material availability, forging
weight and machining content, confirmed with each quotation.

**Who makes these forgings?** Jiangyin Jiangnan Metal Co., Ltd., No.1 Chengxiqiao Road, Zhouzhuang
Town, Jiangyin City, Jiangsu Province, China. Tel +86-189-2135-9659, sales@steelforgepieces.com.

## 11. Enquiry

Send a drawing, a sketch with dimensions, or outside diameter, inside diameter, height and quantity
to sales@steelforgepieces.com, or call +86-189-2135-9659. If the grade is still open, add the
service temperature and medium.