# XM-13 Forgings — ASTM A705 / A564 Type XM-13, UNS S13800, EN 1.4534

**Supplier:** Jiangyin Jiangnan Metal Co., Ltd., integrated steel melting and open-die forging works
**Address:** No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province 214423, China
**Telephone:** 0086-189-2135-9659 · **Email:** sales@steelforgepieces.com
**Canonical page:** https://www.steelforgepieces.com/Stainless-Steel/XM-13.html
**Full property datasheet:** https://www.steelforgepieces.com/Stainless-Steel/PH13-8Mo.html
**Revised:** 11 October 2026

---

## 01 What the designation means

XM-13 is a type designation inside the ASTM age-hardening stainless specifications, not an
alloy name in its own right. It identifies UNS S13800: 12.25 to 13.25 percent chromium,
7.50 to 8.50 percent nickel, 2.00 to 2.50 percent molybdenum and 0.90 to 1.35 percent
aluminium, with carbon at 0.05 percent maximum. The same chemistry carries the PH 13-8 Mo
trademark and the European number 1.4534.

The XM series exists because ASTM needed designations for grades the AISI three-digit system
never covered. A type number is a slot in a specification rather than a standalone standard,
and the same number appears in A564 for bars, A705 for forgings and A693 for flat products,
each with its own testing and acceptance rules. Naming XM-13 alone tells the mill the
chemistry but not the product standard, condition or test regime. Naming ASTM A705 Type
XM-13, H1050, EN 10204 3.1 tells the mill everything.

The alloy hardens by nickel-aluminium intermetallic precipitates rather than carbides, which
is why carbon sits at 0.05 percent maximum. Specified minimum tensile strength runs from
1,517 MPa in H950 to 931 MPa in H1150. Because the carbon, manganese, silicon and sulfur
limits are tight and the steel is vacuum melted, transverse and short-transverse ductility
stay close to the longitudinal values in heavy sections, which is why it appears on
landing-gear and thick valve-part drawings rather than 17-4PH.

### Who supplies the forgings on this page

Jiangyin Jiangnan Metal Co., Ltd. has been melting and forging steel at No.1 Chengxiqiao Road,
Zhouzhuang Town, Jiangyin City, Jiangsu Province, China since 1997. Clean grades such as
UNS S13800 take the vacuum induction and vacuum arc remelting route, with 3 t and 6 t
protective-atmosphere electroslag furnaces also on site. Steel then goes to the 6,300 t,
4,000 t and 2,000 t presses, the 6 m, 3 m and 1 m ring mills, 14 heat-treatment furnaces and
the machine shop without leaving the plant, so one heat number follows the part to the
certificate. 460 staff including 9 senior and 32 intermediate engineers. Approvals from CCS,
BV, DNV, LR and NK.

### Quick reference

| Item | Value |
|---|---|
| Designation | ASTM Type XM-13 |
| UNS number | S13800 |
| Forging specification | ASTM A705 Type XM-13 |
| Bar specification | ASTM A564 Type XM-13 |
| Flat product | ASTM A693 Grade XM-13 |
| Aerospace | AMS 5629 bars, wire, forgings, rings, extrusions |
| Europe | EN 1.4534, X3CrNiMoAl13-8-2 |
| Alloy type | Martensitic precipitation-hardening stainless, nickel-aluminium intermetallics |
| Conditions | A, RH950, H950, H1000, H1025, H1050, H1100, H1150, H1150M |
| Strength range | 931 MPa minimum (H1150) to 1,517 MPa minimum (H950) |
| Hardness range | 30 HRC minimum (H1150) to 45 HRC minimum (H950) |
| Forging range | 1177 to 1204 °C, finish above 954 °C |
| Maximum single piece | 30,000 kg; rolled rings to 6,000 mm outside diameter |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |

---

## 02 Which specification to cite

| Origin | Designation | Scope |
|---|---|---|
| ASTM, forgings | **ASTM A705 Type XM-13** | Age-hardening stainless steel forgings. Cite this on a forging order. |
| ASTM, bars and shapes | ASTM A564 Type XM-13 | Hot-rolled and cold-finished age-hardening bars, rods, shapes |
| ASTM, flat products | ASTM A693 Grade XM-13 | Precipitation-hardening plate, sheet and strip |
| ASTM, listing practice | ASTM A959 | Assigns and lists the XM type designations |
| UNS | UNS S13800 | Unified Numbering System designation, the neutral reference |
| SAE, bars and forgings | **AMS 5629** | Bars, wire, forgings, rings, extrusions. Usual aerospace specification. |
| SAE, flat products | AMS 5864 | Sheet, strip, plate; source of the minimum property table below |
| Trademark | PH 13-8 Mo | Registered trademark of Cleveland-Cliffs Inc. We supply the generic equivalents. |
| Europe | EN 1.4534, X3CrNiMoAl13-8-2 | European material number and name |
| Shop-floor names | 13-8Mo, 13-8 PH, 13/8 Mo, XM13 | Informal names on legacy drawings |
| Does not apply | ASTM B564 | Nickel-alloy forging specification, cited for this grade in error |

*Compiled from ASTM A564, A705, A693 and A959; SAE AMS 5629 and AMS 5864; EN 10088-3;
and mill listings from Rolled Alloys and Universal Stainless.*

### Two errors to watch for

ASTM B564 covers nickel-alloy forgings such as UNS N04400 and N06600 and has nothing to do
with S13800. The correct forging specification is ASTM A705 Type XM-13, or AMS 5629.

The condition H900 does not exist for this grade. It is aged at 950, 1000, 1025, 1050, 1100
or 1150 °F, plus the refrigerated RH950 cycle and the double-aged H1150M cycle. H900, H925
and H1075 belong to 17-4PH. Where a drawing says XM-13 H900 the figures quoted almost always
match H950, but confirm with the designer before the heat is released. An earlier version of
this page carried both errors and they were corrected in October 2026.

---

## 03 Chemical composition, weight percent

| Element | Minimum | Maximum | Function |
|---|---|---|---|
| Carbon | – | 0.05 | Strengthening is by intermetallics, not carbides |
| Manganese | – | 0.10 | One tenth of the 17-4PH limit, suppresses manganese sulfides |
| Silicon | – | 0.10 | Cleanliness and transverse ductility |
| Phosphorus | – | 0.010 | Residual, embrittles grain boundaries |
| Sulfur | – | 0.008 | Tightest limit among the common PH grades |
| Nitrogen | – | 0.010 | Controlled; avoid reducing furnace atmospheres |
| Chromium | 12.25 | 13.25 | Corrosion resistance, martensite stability |
| Nickel | 7.50 | 8.50 | Toughness, partner to aluminium in the strengthening phase |
| Molybdenum | 2.00 | 2.50 | Pitting resistance, solid-solution strengthening |
| Aluminium | 0.90 | 1.35 | The hardening element, forms nickel-aluminium precipitates |
| Iron | Balance | – | Matrix, about 76 percent |

*Rolled Alloys Data Sheet 13-8 Stainless and High Temp Metals PH 13-8 Mo technical data agree
on all limits shown. Published comparisons of the specification families list manganese at
0.20 maximum for ASTM and AMS against 0.10 maximum for EN 1.4534, and aluminium at 0.90 to
1.20 for 1.4534 against 0.90 to 1.35 elsewhere. Confirm manganese and aluminium against the
edition named on the purchase order; either window can be melted.*

No part of this table is reachable by air melting. Carbon at 0.05 percent with silicon at
0.10 percent and sulfur at 0.008 percent needs vacuum induction melting followed by vacuum arc
remelting, which is why most forging shops buy S13800 billet rather than make it.

---

## 04 Conditions and minimum mechanical properties

| Property | H950 | H1000 | H1025 | H1050 | H1100 | H1150 |
|---|---|---|---|---|---|---|
| Aging temperature, °C | 510 | 538 | 552 | 566 | 593 | 621 |
| Yield 0.2 percent, MPa | 1414 | 1310 | 1207 | 1138 | 931 | 621 |
| Yield 0.2 percent, ksi | 205 | 190 | 175 | 165 | 135 | 90 |
| Tensile, MPa | 1517 | 1414 | 1276 | 1207 | 1034 | 931 |
| Tensile, ksi | 220 | 205 | 185 | 175 | 150 | 135 |
| Elongation in 50 mm, percent | 10 | 10 | 11 | 12 | 14 | 14 |
| Reduction of area, longitudinal, percent | 45 | 50 | 50 | 50 | 50 | 50 |
| Reduction of area, short transverse, percent | 35 | 40 | 45 | 45 | 50 | 50 |
| Hardness, minimum | 45 HRC | 43 HRC | – | 40 HRC | 34 HRC | 30 HRC |

*Rolled Alloys Data Sheet 13-8 Stainless, Bulletin 1022USe, tabulating minimum mechanical
properties to AMS 5864. Metric converted at 1 ksi = 6.895 MPa and rounded.*

Two conditions sit outside the table. RH950 cools Condition A material to minus 73 °C for at
least two hours within 24 hours of solution treatment, then ages at 510 °C; the cold hold
clears retained austenite and gives about 1,620 MPa tensile typical at around 48 HRC. H1150M
is a two-stage cycle at 760 then 621 °C, giving the highest impact energy and the best
machinability of the aged conditions.

Solution treatment is 927 °C plus or minus 8 °C, cooled below 16 °C so the structure
transforms fully to martensite. H1150 and H1150M are terminal, so material bought in either
for easier machining has to be re-solution treated before re-aging. Hardness alone will not
separate H1150 from Condition A because the ranges overlap; the certificate is the evidence.

Typical values, torsional data, physical properties and corrosion behaviour are on the
PH13-8Mo page: https://www.steelforgepieces.com/Stainless-Steel/PH13-8Mo.html

---

## 05 Forged shapes and sizes

Three routes: open-die forging for shafts, blocks, discs and tube sheets; seamless ring
rolling for rings from 50 to 6,000 mm outside diameter; upset-and-punch forging for short,
large-section discs and hubs below the ring-mill range.

Shapes supplied: seamless rolled rings, forged rings, gear ring blanks, retaining rings, valve
seat rings, shafts and spindles, eccentric shafts, pins, valve stems, bodies, bonnets and
blocks, discs and blanks, tube sheets, covers, flanges, round and flat bars, blocks, bushings,
sleeves, couplings, hollow cylinders, nozzles and near-net shapes.

Working envelope: single pieces to 30,000 kg on the 6,300 t press; rolled rings to 6,000 mm
outside diameter and from 50 mm by upset and punch; turned shafts to 14,000 mm with 15 m well
furnaces for vertical quenching; machined discs to 5,000 mm swing; deep-hole bored cylinders
to 1,600 × 10,000 mm. For XM-13 the clean-melt ingot governs rather than the press: the 3 t
vacuum induction and 6 t vacuum arc remelting furnaces set the ceiling for double-melt
material.

**Hot working.** Heat uniformly to 1177 to 1204 °C and soak one hour before forging. Do not
forge below 954 °C. Air cool to about 16 °C afterwards. Forgings must be solution treated
before aging. Cold saw bars and billets rather than using an abrasive wheel.

**Machining.** In Condition A, surface speeds run 20 to 30 percent below 17-4PH and 20 to 30
percent below Types 302 and 304. Machinability of the aged conditions improves as the aging
temperature rises, with H1150M the easiest. At 45 HRC and above, turning, drilling and
threading are demanding, so rough in Condition A or H1150M and finish after aging. Aging
produces a small contraction that increases with aging temperature.

Related pages: forged rings (/Forged-Rings/PH13-8Mo-Forged-Rings.html), rolled rings
(/Forging-Rings/PH13-8Mo-Forging-Rings.html), forged shafts (/Forged-Shafts/), forged valve
parts (/Forged-Valve-Parts/), forged tube sheets (/Forged-Tube-Sheets/), forged flanges
(/Forged-Flanges/), forged bars (/Forged-Bars/).

---

## 06 Against the other PH grades

| Grade | UNS | Peak condition | Tensile minimum | Distinguishing feature |
|---|---|---|---|---|
| XM-13 | S13800 | H950 | 1517 MPa | Highest strength of the group, molybdenum and aluminium additions, vacuum melted, short-transverse reduction of area specified separately |
| 17-4PH | S17400 | H900 | 1310 MPa | General industrial grade, lowest cost and widest availability, H1150-M used for sour service |
| 15-5PH | S15500 | – | – | Lower-ferrite variant of 17-4PH for better transverse toughness in heavy forgings. Figures on the 15-5PH page. |
| 17-7PH | S17700 | – | – | Semi-austenitic, formed annealed then transformation hardened. Mainly sheet, strip and spring. |

Start with 17-4PH and move to XM-13 when one of three things is true: the section is heavy and
the drawing calls out transverse or short-transverse properties; the required strength is above
what H900 on 17-4PH will give; or the specification itself names AMS 5629, UNS S13800 or Type
XM-13. The grade costs more and machines harder, and it earns that in those cases.

It is the wrong answer above roughly 593 °C, and long holds between about 288 and 482 °C can
reduce toughness. For strength at temperature rather than at ambient, see A286
(/Stainless-Steel/A286.html).

---

## 07 Testing and certification

Ultrasonic testing to ASTM A388 or EN 10228-3, the part covering ferritic and martensitic steel
forgings, with magnetic particle testing to ASTM E709 and liquid penetrant where specified.
Chemistry by optical emission spectrometry to ASTM E415 with positive material identification,
tensile testing to ASTM A370 and ISO 6892, Charpy V-notch to minus 60 °C, grain size to
ASTM E112. EN 10204 3.1 as standard, EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or your
own inspector on request. The works holds CCS, BV, DNV, LR and NK approvals.

**Sour service.** NACE MR0175 and ISO 15156-3 list precipitation-hardening stainless steels with
named heat-treatment conditions, hardness ceilings and limits on hydrogen sulfide partial
pressure, chloride concentration, pH and temperature. Acceptance is tied to the condition and
the environment, not the grade, and the editions change. Send the hydrogen sulfide partial
pressure, chloride level, pH and maximum temperature with the enquiry.

---

## 08 How to order

Minimum order 10 kg with no minimum piece count. Lead time 20 to 60 days, XM-13 at the upper
end because of the remelting step. Send these six items and a price normally follows within
two working days.

1. **Specification.** ASTM A705 Type XM-13 for forgings, ASTM A564 Type XM-13 for bars,
   AMS 5629 for aerospace, or EN 1.4534. Not ASTM B564.
2. **Melt route.** Single melt, vacuum induction melting plus vacuum arc remelting, or
   electroslag remelted. Double melt is normal for this grade and affects price and lead time.
3. **Dimensions or drawing.** For example 620 mm OD × 420 mm ID × 180 mm high, or a drawing or
   model as PDF, DWG, DXF or STEP with tolerances, surface roughness and grain-flow requirement.
4. **Delivery condition.** Condition A for onward fabrication, H1150M where machining governs,
   or the final aged condition from RH950, H950, H1000, H1025, H1050, H1100 or H1150.
5. **Heat treatment and testing.** For example solution 927 °C then age H1050, ultrasonic to
   EN 10228-3, transverse Charpy at a stated temperature.
6. **Certification and destination.** EN 10204 3.1 or 3.2 with the witnessing body if 3.2, any
   NACE review required, quantity, required date and destination port.

**Contact:** sales@steelforgepieces.com | 0086-189-2135-9659 | WhatsApp https://wa.me/8618921359659
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province 214423, China.
Wuxi Shuofang airport 30 km, Shanghai airports 160 km. Customer audits and third-party
inspection visits are welcome.

---

## 09 Questions

**What is XM-13 stainless steel?**
An ASTM type designation, not an alloy name of its own. It identifies UNS S13800, a martensitic
precipitation-hardening stainless steel of roughly 12.7 Cr, 8 Ni, 2.2 Mo and 1 Al with carbon at
0.05 percent maximum. The same chemistry is sold under the PH 13-8 Mo trademark and listed in
Europe as EN 1.4534.

**Is XM-13 the same as PH13-8Mo?**
Yes, the same chemistry under two naming systems. XM-13 is the ASTM type designation used in
A564, A705 and A693. PH 13-8 Mo is a registered trademark of Cleveland-Cliffs Inc. UNS S13800 is
the neutral number both point to.

**Which ASTM standard covers XM-13 forgings?**
ASTM A705 Type XM-13. A564 covers bars and shapes, A693 covers plate, sheet and strip, AMS 5629
covers aerospace bars, forgings, rings and extrusions. ASTM B564 covers nickel-alloy forgings
and does not apply.

**Does XM-13 have an H900 condition?**
No. The conditions are A, RH950, H950, H1000, H1025, H1050, H1100, H1150 and H1150M. H900, H925
and H1075 belong to 17-4PH.

**What is the strongest condition?**
H950 among the single-step conditions, at 1,517 MPa minimum tensile and 1,414 MPa minimum yield,
45 HRC minimum. RH950 reaches about 1,620 MPa tensile typical at around 48 HRC.

**How large a forging can you make?**
30,000 kg single piece on the 6,300 t press, rolled rings to 6,000 mm outside diameter. For
XM-13 the clean-melt ingot governs: the 3 t vacuum induction and 6 t vacuum arc remelting
furnaces set the ceiling for double-melt material.

**Why does my drawing say 1.4534?**
That is the European material number for the same chemistry, with the name X3CrNiMoAl13-8-2.
The order can be certified to the designation on the purchase order with the equivalents listed
on the same certificate.

---

## 10 Sources

- Rolled Alloys, Data Sheet 13-8 Stainless, Bulletin 1022USe. Chemistry, physical properties,
  heat-treating parameters and minimum mechanical properties to AMS 5864.
- High Temp Metals, PH 13-8 Mo technical data. Cycle definitions, corrosion behaviour,
  workability and machining parameters.
- ASTM A564/A564M Type XM-13; ASTM A705/A705M Type XM-13; ASTM A693 Grade XM-13; ASTM A959.
- SAE AMS 5629 and SAE AMS 5864.
- EN 10088-3 for 1.4534 and X3CrNiMoAl13-8-2; ASTM A388 and EN 10228-3 for ultrasonic testing;
  EN 10204 for certificate types.
- Universal Stainless grade listing, indexing XM-13, PH13-8, 13-8mo, AISI 632, DIN 1.4534 and
  UNS S13800 as the same grade.
- Jiangyin Jiangnan Metal Co., Ltd. equipment register, laboratory register and production
  records for all capability, size, lead-time and certification statements.

Citation: Jiangyin Jiangnan Metal Co., Ltd., XM-13 Forgings, ASTM A705 Type XM-13, UNS S13800,
EN 1.4534, steelforgepieces.com, revised 11 October 2026,