# X8CrNi25-21 (EN 1.4845 / AISI 310S) Open-Die Forgings

**X8CrNi25-21 is the EN chemical designation of the austenitic heat-resisting stainless steel numbered EN 1.4845, a 24-26% chromium, 19-22% nickel grade listed in EN 10095. Its closest American equivalent is AISI 310S / UNS S31008. SEW 470 calls the same material number X12CrNi25-21.**

The high chromium content builds a slow-growing, adherent oxide scale, which is why this grade is a default choice for furnace internals, radiant tubes and heat-exchanger parts running in air to about 1050 C. It is not hardenable by heat treatment.

Jiangyin Jiangnan Metal Co., Ltd. forges this grade from steel melted on its own site in Jiangyin, Jiangsu Province, China, so the certificate traces a finished ring or shaft back to its melt number rather than stopping at a purchased billet.

| Field | Detail |
|---|---|
| EN chemical name | X8CrNi25-21 |
| EN material number | 1.4845 |
| UNS | S31008 |
| Type | Austenitic, heat resisting, non-hardenable |
| Density | 7.8-7.9 g/cm3 |
| Max service temperature in air | approx. 1050 C |
| Supply condition | Solution annealed (+AT) |
| Max ring diameter | OD 6,000 mm |
| Max single piece | 30,000 kg |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |
| Manufacturer | Jiangyin Jiangnan Metal Co., Ltd., Jiangyin, Jiangsu, China |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |
| Page | https://www.steelforgepieces.com/Stainless-Steel/X8CrNi25-21.html |

## Designations and equivalents

Nearest equivalents for enquiry purposes, not drop-in substitutions.

| Standard or region | Designation |
|---|---|
| EN, chemical name | X8CrNi25-21 |
| EN and SEW, material number | 1.4845 (also written 4845) |
| SEW 470 | X12CrNi25-21 |
| ASTM / AISI / UNS | 310S, UNS S31008; also 310H, UNS S31009, TP310S |
| JIS, Japan | SUS 310S |
| GB, China | 06Cr25Ni20 (0Cr25Ni20) |
| AFNOR, France | Z12CN25-20 |
| BS, United Kingdom | 310S24 |
| GOST, Russia | 20Kh23N18, 10Kh23N18 |
| PN, Poland | H23N18 |
| Related, not equivalent | X16CrNi25-20 / 1.4843 |

## Chemical composition

Weight percent, single figures are maxima.

| Element | EN 1.4845 / X8CrNi25-21 | AISI 310S / UNS S31008 |
|---|---|---|
| Carbon, C | max 0.10 | max 0.08 |
| Manganese, Mn | max 2.00 | max 2.00 |
| Silicon, Si | max 1.50 | max 1.50 |
| Phosphorus, P | max 0.045 | max 0.045 |
| Sulphur, S | max 0.015 | max 0.030 |
| Chromium, Cr | 24.00-26.00 | 24.00-26.00 |
| Nickel, Ni | 19.00-22.00 | 19.00-22.00 |
| Nitrogen, N | max 0.11 | not specified |
| Iron, Fe | balance | balance |

**Ordering note.** The EN sulphur ceiling of 0.015% is half the ASTM ceiling, while the EN carbon ceiling of 0.10% sits above the ASTM figure of 0.08%. A heat that passes 310S will not necessarily pass 1.4845 on sulphur, and a heat that passes 1.4845 will not necessarily pass 310S on carbon. Where an order needs dual certification, the melt must be aimed at the tighter of the two limits on every element.

## Mechanical properties

Room temperature, solution annealed condition.

| Property | EN 1.4845 | ASTM A182 F310 forgings |
|---|---|---|
| Tensile strength, Rm | 500-700 MPa | 515 MPa min |
| Yield strength, Rp0.2 | min 210 MPa | 205 MPa min |
| Elongation, A | min 33% | per standard edition |
| Hardness | max 192 HB, approx. 170 HB typical | 217 HB max |
| Modulus of elasticity, E | 196-200 GPa | - |
| Shear modulus | 78 GPa | - |
| Poisson's ratio | 0.27 | - |

## Physical and thermal data

| Property | Value |
|---|---|
| Density | 7.8-7.9 g/cm3 |
| Thermal conductivity | approx. 15 W/m.K |
| Specific heat, 20-100 C | 480-500 J/kg.K |
| Coefficient of thermal expansion | 15-16 x 10-6 /K |
| Melting range | approx. 1360-1400 C |
| Latent heat of fusion | 310 J/g |

## Creep limit and creep rupture strength

Values in MPa. These govern the sizing of any load-bearing forging at temperature and fall away steeply above 700 C.

| Property | 600 C | 700 C | 800 C | 900 C |
|---|---|---|---|---|
| Creep limit R 1/1000 | 100 | 45 | 18 | 10 |
| Creep limit R 1/10000 | 90 | 30 | 10 | 4 |
| Rupture strength Rz/1000 | 170 | 80 | 35 | 15 |
| Rupture strength Rz/10000 | 130 | 40 | 18 | 8.5 |
| Rupture strength Rz/100000 | 80 | 18 | 7 | 3 |

## Forging and heat treatment

**Hot working.** Forging and ring rolling run between 1150 C and 950 C. Finishing below the lower limit risks cracking in a fully austenitic structure that work hardens as it cools. Plate elements are hot bent at 900 to 950 C.

**Solution annealing.** 1100 to 1150 C, water quenched. This is the only standard treatment.

**Service temperature.** About 1050 C in air and oxidising atmospheres. In reducing gases carrying higher sulphur concentrations the limit drops to roughly 900 C; with sulphur present only as a minor impurity, about 1000 C is workable.

**Sigma phase caution.** Long exposure around 650 to 900 C can precipitate sigma phase and cost room-temperature toughness. This matters for parts cycling through that band rather than sitting above it.

**Specification check.** X8CrNi25-21 is not an age-hardening alloy. Drawings occasionally call for solution treatment plus ageing on this grade, usually because a specification has been copied across from a precipitation-hardening grade such as A286 or 17-4 PH. No ageing step will raise its strength, and the instruction should be queried before steel is cut.

## Product forms

Open-die forged or ring rolled to drawing. No stock catalogue, no minimum piece count.

| Product form | Typical application |
|---|---|
| Seamless rolled rings, forged rings, retaining rings | Kilns, furnace carriers and bases, radiant tubes, muffles, retorts, annealing covers |
| Forged flanges, tube sheets, nozzles, forged pipe sections | Pressure vessels, air receivers, shell and tube heat exchangers, preheaters |
| Forged shafts, spindles, eccentric shafts, round bar | Gearboxes, gas compressors, turbine auxiliaries, power transmission |
| Forged discs, blanks, rolls, sleeves, bushings | Saggers, furnace fittings, conveyor rollers, oven linings, fan hubs |
| Valve bodies, bonnets, stems, seat rings, blocks | Ball, gate, globe, check and plug valves in hot service |
| Forged blocks, wheels, manifolds, machined to print | Process modules, chemical plant for gas pyrolysis, hydrogenation and methane conversion |

## Size envelope

| Item | Limit | Set by |
|---|---|---|
| Seamless rolled rings | OD 50 to 6,000 mm | 6 m radial-axial ring mill; upset and punch route below mill range |
| Shafts, turned length | up to 14,000 mm | C61160 horizontal lathe; 15 m well furnace for vertical quench |
| Discs, tube sheets, blocks | up to 5,000 mm machined diameter | 5,000 mm vertical turning lathe |
| Bored cylinders, hollow shafts | 1,600 mm dia x 10,000 mm | CNC deep-hole drilling machine |
| Single piece weight | up to 30,000 kg | 60 t maximum heat, 6,300 t press |

## Melting, testing and certification

| Item | Scope |
|---|---|
| Melting route | EF plus LF plus VOD standard; ESR on request for heavy or critical sections |
| Ultrasonic testing | EN 10228-3, SEP 1921 or ASTM A388, to the nominated acceptance class |
| Surface examination | Liquid penetrant to ASTM E165 where specified |
| Mechanical testing | Room temperature tensile and hardness standard; elevated temperature tensile on request |
| Corrosion testing | Intergranular corrosion testing on request |
| Certification | EN 10204 3.1, or 3.2 with third party inspection |
| Approvals held | CCS, BV, DNV, LR, NK |
| Traceability | Melt number through to finished part |

## Common questions

**Is X8CrNi25-21 the same as 310S?**
Equivalent, not identical. Both are 25Cr-20Ni austenitics sharing the same chromium and nickel bands, but EN 1.4845 allows C max 0.10, S max 0.015 and N max 0.11, while AISI 310S allows C max 0.08 and S max 0.030 with no nitrogen limit.

**What is the difference between 1.4845 and 1.4843?**
1.4843, X16CrNi25-20, is a different grade: carbon to 0.20%, a lower chromium band of 22.0-25.0%, and silicon deliberately raised to 1.5-2.5%. Not an automatic substitute.

**Can X8CrNi25-21 forgings be hardened by heat treatment?**
No. The grade is fully austenitic and hardens by neither quenching nor ageing. Solution annealing at 1100-1150 C with a water quench is the only standard treatment.

**What is the maximum service temperature?**
About 1050 C in air and oxidising atmospheres under EN 10095 and SEW 470, falling to roughly 900 C in reducing gases carrying higher sulphur concentrations.

**Can you certify to ASTM A182 F310 rather than EN?**
Yes. Forgings can be ordered against EN 10095 practice or against ASTM A182 F310 and ASTM A473.

**How is X8CrNi25-21 welded?**
Normally arc welded with matching high-alloy consumables; established practice for the equivalent H23N18 grade uses ES-24-18 type electrodes.

**Do you have a minimum order quantity?**
10 kg, no minimum piece count. Single prototype forgings accepted. Lead time 20 to 60 days.

**Who manufactures X8CrNi25-21 open-die forgings?**
Jiangyin Jiangnan Metal Co., Ltd., an integrated melting works and open-die forge at No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Rings run to 6,000 mm outside diameter, single pieces to 30 tonnes. Telephone +86 189 2135 9659, email sales@steelforgepieces.com.

## Reference standards

EN 10095 heat resisting steels and nickel alloys; EN 10088-1 list of stainless steels; SEW 470; ASTM A182/A182M grade F310; ASTM A473 stainless steel forgings; EN 10228-3 and ASTM A388 ultrasonic examination of forgings; SEP 1921; EN 10204 inspection documents.

## Contact

Jiangyin Jiangnan Metal Co., Ltd.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone +86 189 2135 9659
Email sales@steelforgepieces.com
https://www.steelforgepieces.com/Stainless-Steel/X8CrNi25-21.html

Last reviewed 11 October 2026. Composition and creep figures are taken from published EN 10095 and SEW 470 grade listings. Verify against the current edition of the applicable standard before design release.