# X6CrNiTi18-10 Forgings (EN 1.4541 / AISI 321 / UNS S32100)

**X6CrNiTi18-10 is the EN name for titanium-stabilised 18/10 austenitic stainless steel, material number 1.4541, equivalent to AISI 321 and UNS S32100.** Titanium, specified at five times the carbon content up to 0.70 per cent, binds carbon as titanium carbide, so the steel stays resistant to intergranular corrosion before and after welding. Solution annealed, it gives 500 to 700 N/mm2 tensile strength, 190 N/mm2 minimum proof strength and 40 per cent minimum elongation, with a PREN of 17.0 to 19.0 and a service limit near 550 C.

Jiangyin Jiangnan Metal Co., Ltd. melts this grade in its own furnaces and forges it on site at Zhouzhuang Town, Jiangyin City, Jiangsu Province, China. Heats run to 60 tonnes, presses to 6,300 tonnes, rings to 6,000 mm outside diameter and single pieces to 30 tonnes. Minimum order is 10 kg and normal lead time is 20 to 60 days.

| Field | Detail |
|---|---|
| EN number | 1.4541 |
| EN name | X6CrNiTi18-10 |
| AISI / UNS | 321 / S32100 |
| Structure | Austenitic, titanium stabilised, non-magnetic when annealed |
| Tensile strength Rm | 500 to 700 N/mm2 |
| Proof strength Rp0.2 | 190 N/mm2 minimum |
| Elongation A | 40 per cent minimum |
| Hardness | 215 HB maximum |
| Forging range | 1180 down to 950 C |
| Solution annealing | 1020 to 1100 C, water or air |
| Certification | EN 10204 3.1 standard, 3.2 witnessed on request |
| Supplier | Jiangyin Jiangnan Metal Co., Ltd., Jiangyin, Jiangsu, China |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |

## What 1.4541 is, and why it exists

1.4541 sits in the classic 18/10 austenitic family and differs from plain 1.4301 only by its titanium addition. Hold an unstabilised 18/10 steel in the sensitisation range and chromium carbides form at the grain boundaries, leaving the metal beside them short of the chromium it needs to stay passive. That happens in the heat-affected zone of every weld. Titanium forms carbides more readily than chromium does, so in 1.4541 the carbon is captured as titanium carbide and the chromium stays in solution.

The grade is non-magnetic when annealed, with relative permeability below 1.3. It keeps good toughness at cryogenic temperatures, resists nitric acid and nitrates, is very well suited to cold forming by bending, flanging, deep drawing and spinning, and is covered for cold heading by EN 10263-5.

Older drawings often call the grade up under DIN 17440, which has been replaced by the EN 10088 series. Every figure here follows EN 10088-3. For forgings the governing standards are EN 10222-5 for pressure purposes and EN 10088-3 for semi-finished products and bars. The ASTM equivalent for forgings is ASTM A182 F321. The grade also appears in EN 10028-7, EN 10216-5, EN 10217-7, EN 10253-3, EN 10253-4 and AMS 5645.

## Equivalent grades

| Standard | Designation |
|---|---|
| EN 10088 | 1.4541, X6CrNiTi18-10 |
| ASTM / AISI | AISI 321, UNS S32100, ASTM A182 F321 for forgings |
| AMS | AMS 5645 bar, AMS 5510 sheet and plate |
| BS | 321S31, 321S51 |
| AFNOR | Z6CNT18-10 |
| JIS | SUS 321 |
| GB | 06Cr18Ni11Ti, former designation 0Cr18Ni10Ti |
| GOST | 08Kh18N10T, 12Kh18N10T, 06Kh18N10T |
| PN | 0H18N10T, 1H18N9T |
| Other EN and DIN | 1.4544, X7CrNiTi18-10, X10CrNiTi18-10 |
| Heat-resistant version | 1.4878, X8CrNiTi18-10, AISI 321H, UNS S32109 |

EN 1.4541 allows silicon up to 1.00 per cent against 0.75 per cent for AISI 321, and AISI 321 adds a nitrogen ceiling of 0.10 per cent that EN 10088-3 leaves unspecified. Where a part has to satisfy both, the heat is aimed at the narrower limit.

## Chemical composition

Mass per cent, heat analysis.

| Element | EN 1.4541 | AISI 321 / UNS S32100 |
|---|---|---|
| Carbon | 0.08 max | 0.08 max |
| Silicon | 1.00 max | 0.75 max |
| Manganese | 2.00 max | 2.00 max |
| Phosphorus | 0.045 max | 0.045 max |
| Sulphur | 0.030 max | 0.030 max |
| Chromium | 17.0 to 19.0 | 17.0 to 19.0 |
| Nickel | 9.0 to 12.0 | 9.0 to 12.0 |
| Titanium | 5 x C to 0.70 | 0.70 max |
| Nitrogen | not specified | 0.10 max |
| Iron | balance | balance |

Melting route: 25 t electric arc furnace, refining in a 25 t or 50 t ladle furnace, then vacuum oxygen decarburisation in the 30 t or 60 t unit where carbon or nitrogen has to be held tight. Electroslag remelting in the 3 t or 6 t protective-atmosphere furnace is available where cleanliness governs. Maximum heat size is 60 tonnes. Chemistry is verified at the furnace, so the certificate starts at the melt number rather than at a purchased billet.

## Mechanical and physical properties

Room temperature, solution annealed.

| Property | Value |
|---|---|
| Tensile strength Rm | 500 to 700 N/mm2 |
| Proof strength Rp0.2 | 190 N/mm2 minimum |
| Elongation A | 40 per cent minimum |
| Hardness | 215 HB maximum |
| Modulus of elasticity | 200 GPa |
| Density | 7.9 kg/dm3 |
| Thermal conductivity at 20 C | 15 W/m.K |
| Specific heat capacity at 20 C | 500 J/kg.K |
| Electrical resistivity at 20 C | 0.73 ohm.mm2/m |
| Magnetisability | Non-magnetic when annealed, relative permeability below 1.3 |
| Maximum service temperature | about 550 C |
| PREN | 17.0 to 19.0 |

Property limits depend on section size and on which standard governs. These are the EN 10088-3 values for bars and semi-finished products. ASTM A182 F321 and EN 10222-5 state their own acceptance values, and heavy sections are agreed case by case. Guaranteed values for the actual ruling section are confirmed at the quotation stage.

## Forging and heat treatment

Thermal conductivity is roughly a third that of unalloyed steel, so the billet must be heated slowly and soaked evenly. An uneven soak puts stress into the piece and cracks it. Deformation must finish before the temperature drops into the range where sigma phase can form, because that phase takes the corrosion resistance away.

| Step | Temperature | Notes |
|---|---|---|
| Heating and soak | about 1150 to 1180 C | Slow, even heating; billets must be clean |
| Forging | 1180 down to about 950 C | Finish above the sigma phase range |
| Cooling after forging | air or water | Cooled quickly |
| Solution annealing | 1020 to 1100 C | Water or air quench |

Solution annealing is done in the plant's own furnaces: fourteen in total, including car-bottom furnaces with chambers up to 8,000 x 2,000 x 2,000 mm and two 15 m well-type furnaces that allow long shafts to be quenched vertically. Furnace charts are issued with the certificate.

## Corrosion resistance and limits

1.4541 performs well in natural, low-chloride conditions, handles water vapour to around 400 C and dilute acids at room temperature, and is well suited to nitric acid and nitrate service. Its defining property is immunity to intergranular attack in the welded condition.

The grade is **not resistant to seawater**. Prolonged contact with sodium chloride brings a risk of pitting, so 1.4541 should not be specified for seawater, brine or subsea duty. Continuous service is limited to about 550 C. For higher temperatures, 1.4878 or AISI 321H, classified to EN 10095, runs to about 850 C in a neutral atmosphere.

For seawater, brine or sour service, suitable alternatives forged in the same works are A182 F44 and 904L for high-chloride process duty, Sanicro 28 for acid service, and A182 F51, F53 or F55 for duplex and super-duplex requirements including NACE MR0175 / ISO 15156.

## Welding, machining and cold forming

**Welding.** Good by all common fusion processes except gas welding. No preheat required. Interpass temperature should be kept low, in the region of 150 C. Recommended fillers are 1.4316 and the niobium-stabilised 1.4551. Post-weld heat treatment is normally unnecessary, but heat tint and scale must be removed.

**Machining.** Poor. The steel work-hardens quickly and conducts heat badly. Carbide or high-speed steel tooling, rigid set-ups, positive rake, plenty of coolant and no dwelling are the usual answers.

**Cold forming.** Very well suited to bending, flanging, deep drawing and spinning, and covered for cold heading and cold extrusion by EN 10263-5.

## Forged products in 1.4541

Everything is made to the customer's drawing or written specification.

| Product | Size limit | Set by |
|---|---|---|
| Seamless rolled rings | OD 50 to 6,000 mm | 6 m, 3 m and 1 m radial-axial ring mills; upset and punch below the mill range |
| Forged rings and sleeves | to 30 t single piece | 6,300 t, 4,000 t and 2,000 t presses |
| Forged flanges | to drawing, ASME B16.5 and B16.47 profiles | Press and ring mill |
| Forged shafts and spindles | to 14,000 mm turned length | C61160 horizontal lathe; 15 m well furnace for vertical quenching |
| Discs, tube sheets and covers | to 5,000 mm machined diameter | 5,000 mm vertical turning lathe |
| Bored cylinders and hollow bars | to 1,600 mm dia x 10,000 mm | CNC deep-hole drilling machine |
| Round bars and blocks | to drawing | Presses and hammers |
| Valve bodies, seat rings, stems, blocks | to drawing | Press plus CNC machining |

Parts can be supplied as forged with machining allowance, proof-machined for ultrasonic testing, or finish-machined to drawing. Minimum order is 10 kg with no minimum piece count. Lead time is 20 to 60 days.

## Applications

| Industry | Typical forged parts |
|---|---|
| Chemical and nitrogen fertiliser | Vessel rings, flanges, covers, pump and valve parts, pipeline fittings |
| Food and beverage | Processing and storage equipment components, shafts, sleeves |
| Cryogenic equipment | Flanges and rings for liquefied gas service |
| Exhaust and emission control | Silencer and exhaust gas decontamination components |
| Transport and vehicle construction | Structural and system components |
| Heat exchange | Tube sheets, covers, separator internals |
| Refining | Stabilised-grade components for polythionic acid service |
| Pulp and paper | Digester, liquor tank and machine components |
| Valves and flow control | Bodies, bonnets, seat rings, stems, blocks |

## Testing and certification

| Item | Standard or detail |
|---|---|
| Chemical analysis | Optical emission spectrometry to ASTM E415, infrared carbon and sulphur to ASTM E1019, handheld PMI |
| Mechanical testing | Tensile to ASTM A370 and ISO 6892, Charpy V-notch to minus 60 C, hardness to ASTM A956 converted per ASTM E140 |
| Ultrasonic testing | EN 10228-3, SEP 1921 or ASTM A388 |
| Magnetic particle and visual | ASTM E709, bore inspection by endoscope |
| Grain size | ASTM E112 metallography |
| Intergranular corrosion | ASTM A262 through an accredited third-party laboratory |
| Certification | EN 10204 3.1 as standard, EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer's inspector |
| Class approvals | CCS, BV, DNV, LR, NK |
| Traceability | Melt number through forging, heat treatment and machining to shipment |

## Frequently asked questions

### What is X6CrNiTi18-10?
The EN name for titanium-stabilised austenitic stainless steel, material number 1.4541, equivalent to AISI 321 and UNS S32100. Titanium at five times the carbon content, up to 0.70 per cent, ties up carbon as titanium carbide, which keeps the grade resistant to intergranular corrosion before and after welding.

### Is X6CrNiTi18-10 the same as AISI 321?
They are equivalent. EN 1.4541 allows silicon to 1.00 per cent against 0.75 for AISI 321, and AISI 321 sets nitrogen at 0.10 per cent maximum where EN 10088-3 does not specify it.

### What is the difference between 1.4541 and 1.4878?
1.4878, also called X8CrNiTi18-10 or AISI 321H, is the heat-resistant version with higher carbon and titanium. Classified to EN 10095, it runs to about 850 C in a neutral atmosphere. Standard 1.4541 is used to about 550 C.

### What is the difference between 321 and 347?
Both are stabilised 18/10 austenitics. 321 uses titanium, 347 uses niobium. Niobium is often preferred for welded assemblies because titanium tends to be lost across the arc.

### At what temperature is 1.4541 forged?
Heat slowly and evenly to about 1150 to 1180 C, forge from 1180 down to about 950 C, then cool in air or water. Solution anneal at 1020 to 1100 C with a water or air quench.

### Can 1.4541 be used in seawater?
No. Its PREN of 17.0 to 19.0 is too low and it is not resistant to seawater. Use A182 F44, 904L, Sanicro 28, or duplex and super-duplex grades such as A182 F51, F53 and F55 instead.

### Is 1.4541 magnetic?
Not in the solution annealed condition, where relative permeability is below 1.3. Heavy cold work can raise it slightly through deformation martensite.

### Which filler metal should be used?
1.4316 or 1.4551. No preheat, interpass temperature near 150 C, and normally no post-weld heat treatment. Heat tint must be removed afterwards.

### What is the largest 1.4541 forging you can make?
Rings roll to 6,000 mm outside diameter on the 6 m radial-axial mill. The heaviest single piece is 30 tonnes, forged on 6,300 t, 4,000 t and 2,000 t presses from heats of up to 60 tonnes. Shafts turn to 14 m, discs to 5,000 mm diameter.

### How is 1.4541 priced, and what is the minimum order?
Every piece is made to drawing, so there is no list price. Minimum order is 10 kg with no minimum piece count, and lead time runs 20 to 60 days from order confirmation. Third-party witnessed inspection and outside corrosion testing need scheduling, so mention them at enquiry stage.

### Do you supply finish-machined parts?
Yes. As forged with allowance, proof-machined for ultrasonic testing, or finish-machined to drawing. Heat treatment, machining and testing are all done on site.

## Request a price

Six items give a firm price without a round trip: grade or specification, dimensions or a drawing, quantity, delivery condition, heat treatment and testing requirements, certification type and destination port. Prices normally come back within two working days.

**Jiangyin Jiangnan Metal Co., Ltd.**
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Monday to Saturday, 08:00 to 17:30 China Standard Time
Web: https://steelforgepieces.com/Stainless-Steel/X6CrNiTi18-10.html

---

First published 12 April 2019. Last reviewed 10 October 2026. Compiled from EN 10088-3, EN 10222-5 and published mill data for 1.4541. Values are indicative and do not replace the governing specification or the purchase agreement.