# X4CrNiMo16-5-1 Forgings (EN 1.4418)

**X4CrNiMo16-5-1, material number 1.4418, is a soft martensitic chromium-nickel-molybdenum stainless steel.** Carbon is held below 0.06 per cent, which is what separates it from the older 13 per cent chromium martensitics. The low carbon produces a tough, weldable martensite instead of a hard and brittle one, and leaves enough free chromium in solution to resist intergranular attack. Nickel at 4 to 6 per cent stabilises the structure and holds up impact toughness down to cryogenic temperatures. Molybdenum at around 1 per cent lifts pitting resistance far enough for limited marine exposure. Quenched and tempered to QT900 the grade reaches 900 to 1100 N/mm2 tensile strength, which is why it ends up in pump shafts, centrifuge bodies and water turbine parts where load and corrosion arrive together.

Jiangyin Jiangnan Metal Co., Ltd. forges this grade as rings, bars, discs, hollow sections and shafts at an integrated melting and open-die forging works in Zhouzhuang Town, Jiangyin City, Jiangsu Province, China.

Source page: https://www.steelforgepieces.com/Stainless-Steel/X4CrNiMo16-5-1.html

## Grade summary

| Field | Value |
|---|---|
| EN designation | X4CrNiMo16-5-1 |
| Material number | 1.4418 |
| Structure | Soft martensitic, ferromagnetic |
| Composition | C max 0.06, Cr 15.00 to 17.00, Ni 4.00 to 6.00, Mo 0.80 to 1.50, N min 0.02 |
| PRE | 17.95 to 22.27 |
| Density | 7.70 kg/dm3 |
| Delivery conditions | Soft annealed, QT760, QT900 |
| Service temperature | Cryogenic up to around 550 C |
| Governing forging standard | EN 10250-4 |
| Certification | EN 10204 3.1 or 3.2 |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |

## Chemical composition

The grade name encodes the aim analysis: roughly 16 per cent chromium, 5 per cent nickel, 1 per cent molybdenum, with the leading 4 standing for 0.04 per cent carbon. Iron is the balance.

| C | Si | Mn | P | S | Cr | Ni | Mo | N |
|---|---|---|---|---|---|---|---|---|
| max 0.06 | max 0.70 | max 1.50 | max 0.040 | max 0.030 | 15.00 to 17.00 | 4.00 to 6.00 | 0.80 to 1.50 | min 0.02 |

Some mill specifications tighten sulphur to 0.015 per cent maximum where polishability or transverse toughness governs. State the requirement on the enquiry and it is set at the ladle furnace rather than screened for afterwards.

## Designations and standards

The grade runs through the full set of EN stainless standards. For forgings the governing document is EN 10250-4, open steel die forgings for general engineering purposes, stainless steels. It also appears in EN 10088-1 through EN 10088-5, in EN 10272 for bars for pressure purposes and in EN 10028-7 for flat products for pressure purposes.

| System | Designation |
|---|---|
| EN / DIN | 1.4418, X4CrNiMo16-5-1, X 4 CrNiMo 16-5-1 |
| AFNOR, France | Z6CND16-05-01 |
| AIR 9160, aerospace | Z8CND17.04, Z8CND17-04 |
| SIS / SS, Sweden | SS 2387, S165M |
| Works and trade names | X164M, BMS H-10, 248SV, FE-PM3504 |
| GOST type, CIS | 08Kh17N5M3 |

### It is not F6NM

There is no exact ASTM or UNS twin for 1.4418. ASTM A182 F6NM and UNS S41500 correspond to EN 1.4313, X3CrNiMo13-4, which runs about 13 per cent chromium and 4 per cent nickel. X4CrNiMo16-5-1 runs about 16 per cent chromium, 5 per cent nickel and 1 per cent molybdenum, so it sits a clear step above F6NM on corrosion resistance. Both are soft martensitic grades aimed at pump and hydro turbine duty, and buyers substitute one for the other more often than they should. We forge both and will not swap one for the other without written approval.

## Mechanical properties

Two quenched and tempered levels are normally specified, named after their minimum tensile strength. QT900 is the condition industry orders most often. Tempering temperature is chosen to hit the required level rather than fixed by the grade.

| Condition | Rp0.2 N/mm2 | Rm N/mm2 | A5 % | ISO-V at 25 C | Hardness |
|---|---|---|---|---|---|
| Soft annealed | - | max 1100 | - | - | max 320 HB |
| QT760, specified | min 550 | 760 to 960 | min 16 | min 90 J | - |
| QT760, typical | 820 | 940 | 18 | - | - |
| QT900, specified | min 700 | 900 to 1100 | min 16 | min 80 J | - |
| QT900, typical | 920 | 1050 | 18 | - | - |

At 160 mm ruling section and above, the property level has to be agreed between purchaser and manufacturer, because hardening response falls off toward the centre of a heavy forging. On rings and discs we take test pieces from a prolongation representing the heaviest section and quote the achievable level before the order is confirmed.

Minimum proof strength at elevated temperature is specified in EN 10088-3 for both conditions and declines steadily with temperature. Ask for the figures against your service temperature.

## Physical properties

| Property | Value |
|---|---|
| Density | 7.70 kg/dm3 |
| Thermal conductivity at 20 C | 15 W/m.K |
| Specific heat capacity at 20 C | 430 J/kg.K |
| Electrical resistivity at 20 C | 0.70 ohm.mm2/m |
| Magnetisable | Yes, ferromagnetic in all conditions |
| Thermal expansion 20 to 100 C | 10.8 x 10-6 per K |
| Thermal expansion 20 to 200 C | 10.8 x 10-6 per K |
| Thermal expansion 20 to 300 C | 11.2 x 10-6 per K |
| Thermal expansion 20 to 400 C | 11.6 x 10-6 per K |

## Corrosion behaviour

Pitting resistance equivalent falls between 17.95 and 22.27 depending where the analysis sits inside the specification band. That puts 1.4418 well above 1.4057, and the molybdenum addition allows limited exposure to marine environments.

In most media the general corrosion resistance is about the level of AISI 304L. The useful part is what the low carbon and the microstructure buy on top of that: the grade is highly resistant to intergranular corrosion, to corrosion fatigue and to stress corrosion cracking, and it keeps that resistance across a weld. For a shaft running in water under alternating load, resistance to corrosion fatigue matters more than a general corrosion rate, which is the reason this grade displaced plain 13 per cent chromium steels in hydraulic machinery.

Finished surfaces have to be free of scale, lubricant and embedded iron before the part goes into service. Where a forging has been machined on tooling that also cuts carbon steel, specify passivation and it will be carried out and recorded.

## Forging

Heat the stock gradually to about 800 C before raising it more quickly to between 1150 C and 1180 C. Forge between 1180 C and 950 C. Cool in a furnace, in dry ash or under an equivalent insulating medium. The grade air hardens, so a heavy section cooled in still air straight from the press can crack before it reaches the heat treatment bay.

## Heat treatment

| Operation | Temperature | Cooling |
|---|---|---|
| Soft annealing | Around 600 C, not above 625 C | Slow cool in air |
| Hardening | 1000 to 1050 C | Air, oil or polymer |
| Tempering | Selected to reach QT760 or QT900 | See restriction below |

The band from 420 C to 510 C must be traversed rapidly. Do not temper inside it and do not slow cool through it. Before final tempering the piece must already have cooled right through to below 40 C, otherwise transformation to martensite is incomplete and the tempered structure will not be uniform. On heavy rings and shafts this is the step most often skipped, and it shows up later as scattered impact results.

## Welding

1.4418 is readily weldable by all standard techniques and holds its strength and corrosion resistance across the joint. Preheat the workpiece to between 100 C and 200 C. Do not use hydrogen or carbon bearing gases when welding under shielding gas. Anneal or temper the weldment afterwards. Use a matching filler, or a 1.4430 type filler where a dissimilar consumable is acceptable.

## Machining

Machinability is the weak point of the grade and tracks hardness directly, cutting much like a carbon steel at the same hardness. The grade takes a good polish, which suits shafts running in seals.

| Depth of cut | Feed rate | Cutting speed |
|---|---|---|
| 1 mm | 0.2 mm/rev | 135 m/min |
| 3 mm | 0.4 mm/rev | 100 m/min |
| 6 mm | 0.5 mm/rev | 95 m/min |

Guideline for tempered material, Rm 900 to 1150 N/mm2.

## Applications

X4CrNiMo16-5-1 gets specified when a part is mechanically loaded and corrosion exposed at the same time, and when a casting or a plain martensitic steel has already failed at one of the two. Established applications are pump shafts and spindles, disc stack and decanter centrifuge bowls, bodies and hood covers, water turbine and Kaplan turbine components, marine propeller shafting, valve bodies and trim, injector bodies, compressor components, crankshafts, pistons, pins, agitators and highly stressed bolting.

By sector that lands in chemical processing, hydro and thermal power generation, shipbuilding and marine, general mechanical engineering, and aviation and aerospace, where the AIR 9160 designation Z8CND17.04 covers it.

## Product forms supplied in this grade

Every piece is forged from steel melted in our own furnaces. Nothing is cast, nothing is welded up from sections, and no billet of unknown origin enters the route.

- Seamless rolled rings to 6,000 mm outside diameter, rectangular or contoured section. Upset and punched forged rings from OD 50 mm for sections outside the mill envelope.
- Forged round, flat, square and hexagonal bars, blocks and billets.
- Solid forged discs, plates and covers up to 5,000 mm machined diameter, proof-machined where volumetric inspection is required.
- Hollow bars, sleeves, bushings, cylinders, casings, hubs and housings bored from solid forged blanks, up to 1,600 mm diameter by 10,000 mm.
- Pump shafts, stepped shafts and spindles up to 14,000 mm turned length, quenched vertically in 15 m well-type furnaces.
- Turbine blade blanks, centrifuge bowl bodies and hood covers, and other near-net components forged to drawing.

| Order parameter | Value |
|---|---|
| Maximum single piece | 30,000 kg |
| Maximum ring diameter | 6,000 mm OD |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days from order confirmation |
| Delivery condition | Soft annealed, QT760 or QT900; as-forged, proof-machined or finish-machined |

## Testing and certification

Because the steel is melted here, chemistry is verified at the furnace rather than copied from a supplier certificate, and the melt number follows the part through forging, heat treatment and machining to shipment.

Forged rings and components are ultrasonically tested to EN 10228-3 or ASTM A388 against the acceptance class nominated. Composition is confirmed by optical emission spectrometry to ASTM E415 and by handheld PMI. Tensile testing runs on 600 kN and 300 kN machines to ASTM A370 and ISO 6892, and Charpy V-notch impact testing is available to minus 60 C in house. Magnetic particle inspection to ASTM E709 applies, since the grade is ferromagnetic.

Intergranular corrosion testing to ASTM A262 or ASTM G28 and pitting tests to ASTM G48 are placed with an accredited third-party laboratory and the report is issued alongside the mill certificate.

EN 10204 3.1 mill test certificates are standard. EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer's own inspector is available on request. The works holds CCS, BV, DNV, LR and NK approvals.

## Frequently asked questions

### What is X4CrNiMo16-5-1 steel?

A soft martensitic chromium-nickel-molybdenum stainless steel, material number EN 1.4418, containing max 0.06 per cent carbon, 15.00 to 17.00 per cent chromium, 4.00 to 6.00 per cent nickel, 0.80 to 1.50 per cent molybdenum and min 0.02 per cent nitrogen. The low carbon keeps the martensite tough and weldable, and makes the grade highly resistant to intergranular corrosion, corrosion fatigue and stress corrosion cracking.

### Is 1.4418 the same as F6NM or UNS S41500?

No. F6NM and UNS S41500 correspond to EN 1.4313, X3CrNiMo13-4, at about 13 per cent chromium and 4 per cent nickel. X4CrNiMo16-5-1 runs about 16 per cent chromium, 5 per cent nickel and 1 per cent molybdenum, so its corrosion resistance is higher. They are separate specifications and should not be substituted without engineering approval. There is no exact ASTM or UNS equivalent for 1.4418.

### What strength does the grade reach?

QT760 gives min 550 N/mm2 proof strength, 760 to 960 N/mm2 tensile strength, min 16 per cent elongation and min 90 J impact energy, typically measuring 820 N/mm2, 940 N/mm2 and 18 per cent. QT900 gives min 700 N/mm2 proof strength, 900 to 1100 N/mm2 tensile strength, min 16 per cent elongation and min 80 J, typically measuring 920 N/mm2, 1050 N/mm2 and 18 per cent. Above 160 mm ruling section the level has to be agreed before order.

### Is X4CrNiMo16-5-1 magnetic?

Yes. It is ferromagnetic in every delivery condition, unlike austenitic grades such as 304 and 316. That allows magnetic particle inspection, and it rules the grade out where a non-magnetic part is required.

### Can it be used at low temperature?

Yes. The grade is used in cryogenic applications and holds useful toughness at low temperature, which is one of its advantages over conventional 13 per cent chromium martensitic steels. At the top end it can be used to around 550 C. Impact testing to minus 60 C is carried out in our own laboratory; below that it is placed with an accredited third-party laboratory.

### How should it be forged?

Heat gradually to about 800 C, then more rapidly to between 1150 C and 1180 C. Forge between 1180 C and 950 C, then cool slowly in a furnace or in dry ash. Cooling a heavy section in still air straight from the press risks cracking, because the grade air hardens.

### Can it be welded?

Yes, by all standard techniques, and it holds its strength and corrosion resistance across the joint. Preheat to between 100 C and 200 C, avoid hydrogen or carbon bearing gases under shielding gas, and anneal or temper the weldment afterwards. Use a matching filler or a 1.4430 type filler.

### What is the minimum order and the lead time?

Minimum order is 10 kg with no minimum piece count, so a single prototype ring or shaft is quotable. Lead time runs 20 to 60 days from order confirmation. Witnessed inspection to EN 10204 3.2 and third-party corrosion testing both need scheduling, so flag them at enquiry stage.

## Request a quotation

Send the grade and condition, the dimensions or a drawing in PDF, DWG, DXF or STEP, the quantity, the delivery condition, the testing and certification requirements and the destination port.

| # | Item | Example |
|---|---|---|
| 1 | Material grade and condition | X4CrNiMo16-5-1 / 1.4418, QT900 |
| 2 | Dimensions or drawing | OD 980 x ID 720 x H 240 mm, seamless rolled ring |
| 3 | Quantity and repeat volume | 8 pcs, twice a year |
| 4 | Delivery condition | Proof-machined, 6 mm allowance all faces |
| 5 | Testing requirements | UT to EN 10228-3 class 3, Charpy at -20 C |
| 6 | Certification and destination | EN 10204 3.2 witnessed by DNV, Rotterdam |

**Jiangyin Jiangnan Metal Co., Ltd.**
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Business hours: Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8)
Web: https://www.steelforgepieces.com/Stainless-Steel/X4CrNiMo16-5-1.html

## Data sources and revision

Composition, physical and mechanical data follow EN 10088-3 and published mill data sheets for material 1.4418. Forging, heat treatment, welding and machining parameters follow the Deutsche Edelstahlwerke data sheet for 1.4418, revision 4418-1. Standards covering the grade are EN 10088-1, EN 10088-2, EN 10088-3, EN 10088-4, EN 10088-5, EN 10028-7, EN 10272 and EN 10250-4. Page last reviewed 10 October 2026.

Figures are given in good faith for guidance and do not form a warranty. Acceptance values for a specific order are confirmed against the governing specification at the quotation stage.

---
