# X3CrNiMoAl13-8-2 Forgings (1.4534 / UNS S13800 / PH 13-8 Mo)

**X3CrNiMoAl13-8-2, EN material number 1.4534, is a martensitic precipitation-hardening stainless steel with 12.25 to 13.25 per cent chromium, 7.5 to 8.5 per cent nickel, 2.0 to 2.5 per cent molybdenum and 0.90 to 1.35 per cent aluminium. It is the European designation of UNS S13800, sold as PH 13-8 Mo and covered by ASTM grade XM-13 and AMS 5629.**

The alloy reaches 1515 MPa minimum tensile strength in the H950 condition while keeping transverse properties close to longitudinal ones, which is why it is chosen over other precipitation-hardening grades for thick forged sections in subsea, valve, aerospace and pump service.

Jiangyin Jiangnan Metal Co., Ltd. melts this grade on site and forges it in the same works. Sulphur is limited to 0.008 per cent and phosphorus to 0.010 per cent, so the heat is refined under vacuum and remelted by electroslag or vacuum arc remelting rather than bought in as billet.

## Supplier record

| Field | Detail |
|---|---|
| Manufacturer | Jiangyin Jiangnan Metal Co., Ltd. |
| Plant | No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China |
| Established | 1997 |
| Business | Integrated melting works, open-die forge and ring rolling mill |
| Melt route for this grade | EF + LF + VOD, remelted by ESR or VAR. 60 t maximum heat |
| Forging | 6,300 t, 4,000 t and 2,000 t presses; ring mills at 6 m, 3 m and 1 m; 30 t maximum single piece |
| Heat treatment | 14 furnaces, car-bottom to 8,000 x 2,000 x 2,000 mm, two 15 m well-type furnaces |
| Approvals | CCS, BV, DNV, LR, NK |
| Certification | EN 10204 3.1 standard, EN 10204 3.2 witnessed on request |
| Minimum order | 10 kg, no minimum piece count |
| Lead time | 20 to 60 days |
| Telephone | +86 189 2135 9659 |
| Email | sales@steelforgepieces.com |
| Page | https://steelforgepieces.com/Stainless-Steel/X3CrNiMoAl13-8-2.html |

## 1. Designations and equivalents

| Standard or system | Designation |
|---|---|
| EN / Werkstoff | X3CrNiMoAl13-8-2, 1.4534 |
| UNS | S13800 |
| ASTM | A564 XM-13, A693 XM-13, A705 XM-13, A959 XM-13 |
| AMS | AMS 5629 |
| Trade names | PH 13-8 Mo, 13-8 Mo, Marval X12 |
| British | BS 13-8, N709 |
| French (AFNOR) | Z1CNDA12-09, Z4CNDAT13-09, X1CrNiMoAl12-9 |
| Chinese | 04Cr13Ni8Mo2Al |

Neighbouring grades forged in the same shop: PH 13-8 Mo, 17-4 PH, 17-7 PH, 15-5 PH.

## 2. Chemical composition

Weight per cent. ASTM XM-13 and UNS S13800 limits, with EN 1.4534 variations in the last column.

| Element | Minimum | Maximum | EN 1.4534 variation |
|---|---|---|---|
| Carbon, C | - | 0.05 | |
| Silicon, Si | - | 0.10 | |
| Manganese, Mn | - | 0.20 | 0.10 maximum |
| Phosphorus, P | - | 0.010 | |
| Sulphur, S | - | 0.008 | |
| Chromium, Cr | 12.25 | 13.25 | |
| Nickel, Ni | 7.50 | 8.50 | |
| Molybdenum, Mo | 2.00 | 2.50 | |
| Aluminium, Al | 0.90 | 1.35 | 0.90 to 1.20 |
| Nitrogen, N | - | 0.010 | |
| Iron, Fe | Balance, about 76 | | |

Aluminium is the hardening element; it forms the fine NiAl precipitate that gives the alloy its strength on ageing. The sulphur and phosphorus limits cannot be met by arc melting alone, which is why the grade is normally double melted.

Chemistry is verified at the furnace on a SPECTROTEST TXC25 optical emission spectrometer to ASTM E415, with carbon and sulphur confirmed on an infrared analyser to ASTM E1019.

## 3. Mechanical properties

### Specified minima, ASTM A564 grade XM-13

| Condition | Tensile, MPa | 0.2% proof, MPa | Elongation, % | HRC | HB |
|---|---|---|---|---|---|
| A, solution treated | - | - | - | 38 max | 363 max |
| H950 | 1515 | 1415 | 10 | 45 | 450 |
| H1000 | 1415 | 1310 | 10 | 43 | 400 |
| H1025 | 1280 | 1210 | 11 | 41 | 380 |
| H1050 | 1210 | 1140 | 12 | 40 | 372 |
| H1100 | 1035 | 950 | 14 | 34 | 313 |
| H1150 | 930 | 620 | 14 | 30 | 283 |
| H1150M | 860 | 585 | 16 | 26 | 259 |

### Typical longitudinal values

| Condition | 0.2% proof, MPa | Tensile, MPa | Elongation in 50 mm, % | Reduction of area, % | HRC | CVN, J |
|---|---|---|---|---|---|---|
| RH950 | 1482 | 1620 | 12 | 45 | 48 | 27 |
| H950 | 1449 | 1551 | 12 | 50 | 47 | 27 |
| H1000 | 1413 | 1482 | 13 | 55 | 45 | 41 |
| H1050 | 1241 | 1310 | 15 | 55 | 43 | 68 |
| H1100 | 1034 | 1103 | 18 | 60 | 35 | 81 |
| H1150 | 724 | 1000 | 20 | 63 | 33 | 103 |
| H1150M | 586 | 896 | 22 | 70 | 32 | 163 |

Transverse values stay close to longitudinal ones. A typical transverse test in H950 gives about 1448 MPa proof strength and 1551 MPa tensile at 12 per cent elongation. For a ring or a heavy disc, where the critical stress often runs across the grain flow, that is the property that decides the grade.

Tensile testing runs in house on a 600 kN WE-600B machine and a WDW-300 electronic machine to ASTM A370 and ISO 6892. Charpy impact testing uses a JBN-300 pendulum with a DWC-60 low-temperature bath, down to minus 60 degrees Celsius.

## 4. Physical properties

| Property | Value | Condition or temperature |
|---|---|---|
| Density | 7.76 to 7.8 g/cm3 | H1000, room temperature |
| Modulus of elasticity | 195 to 203 GPa | room temperature |
| Modulus of rigidity | 76.5 GPa | H950 |
| Poisson's ratio | 0.27 to 0.30 | room temperature |
| Thermal conductivity | 14 to 15 W/m.K | condition A, 100 C |
| Specific heat capacity | about 500 J/kg.K | 20 C |
| Mean thermal expansion | 10.6 x 10-6 /K | H950, 21 to 93 C |
| Electrical resistivity | about 1020 micro-ohm.mm | condition A, 100 C |
| Magnetic response | Ferromagnetic | all conditions |
| Service temperature | high strength held to about 315 C; oxidation resistance to about 595 C | - |

Design note: long exposure between roughly 288 and 482 C can lower toughness in precipitation-hardening stainless steels. Ageing at a higher temperature reduces the effect, and service excursions should stay at least 28 C below the ageing temperature used.

## 5. Heat treatment conditions

| Condition | Cycle |
|---|---|
| A | 927 C plus or minus 8 C, hold to section, cool below 16 C to complete transformation to martensite. Sections under about 230 cm2 may be liquid quenched; heavier sections air cool |
| RH950 | From condition A: minus 73 C for at least 2 hours within 24 hours of solution treatment, warm in air, then 510 C plus or minus 6 C for 4 hours, air cool |
| H950 | 510 C for 4 hours, air cool |
| H1000 | 538 C for 4 hours, air cool |
| H1025 | 552 C for 4 hours, air cool |
| H1050 | 566 C for 4 hours, air cool |
| H1100 | 593 C for 4 hours, air cool |
| H1150 | 621 C for 4 hours, air cool |
| H1150M | 760 C for 2 hours, air cool, then 621 C for 4 hours, air cool. Best machinability of the aged conditions |

Two traps worth avoiding. H900 belongs to 17-4 PH and does not exist for this grade; 510 C, giving H950, is as low as the ageing goes. And material delivered in H1150 or H1150M will not respond to further ageing until it has been re-solution treated at 927 C, and hardness alone will not tell the two apart because the H1150 range overlaps the solution-treated range.

Ageing contracts the part predictably: roughly 0.0004 to 0.0006 mm per mm for H950 and H1000, 0.0005 to 0.0008 for H1050, and 0.0008 to 0.0012 for H1100.

## 6. Forging, machining and welding

**Forging.** Heat to 1177 to 1204 C and soak about an hour at temperature. Stop forging at 955 C. Air cool below about 16 C, then solution treat before any ageing. Remove scale by grit blasting or acid cleaning and passivate finished surfaces.

**Machining.** In condition A the grade cuts cleanly but at speeds roughly 20 to 30 per cent below 17-4 PH or type 302 and 304 stainless. Machinability improves as ageing temperature rises, and H1150M is the easiest aged condition. At H950 the material sits near 47 HRC. For parts with heavy machining content, supply in condition A or H1150M and age afterwards. Cold saw rather than abrasive cut, which can leave fine surface cracks on annealed stock.

**Welding.** Inert-gas shielded and resistance processes both work, normally on solution-annealed material with 13-8 Mo filler, and preheat is not usually needed. Where full weld strength is not required, E308L or ER308L can be used. Design out sharp corners, threads and partial-penetration joints. Solution treat the welded assembly before ageing for the best combination of strength, ductility and corrosion resistance.

## 7. Corrosion behaviour

In the H950 condition the alloy resists rusting in 5 per cent salt fog about as well as type 304, and its general corrosion resistance in oxidising and reducing acids and in open-air exposure comes close to 304. Resistance is highest fully hardened and falls slightly as ageing temperature rises.

Marine-atmosphere testing shows a high level of resistance to stress-corrosion cracking in both wrought and welded material. Where cracking is the governing risk, ageing at 538 C or above is the usual recommendation. The grade also behaves well against sodium chloride, nitric acid and sodium hydroxide. Surfaces must be free of scale and embedded iron, and finished parts passivated.

## 8. Forgings supplied in this grade

Every item is forged from a single piece of steel melted on site. No welding, no casting, no purchased billet of unknown origin.

- **Seamless rolled rings.** Ring-rolled from a punched preform on a radial-axial mill, rectangular or contoured section.
- **Forged rings.** Upset and punched, for sections outside the ring-mill envelope and where heavy reduction is wanted.
- **Forged shafts and spindles.** Stepped, eccentric and crankshaft forms, quenched vertically in the well furnaces where length demands it.
- **Forged flanges.** Weld neck, blind, slip-on, long weld neck and special profiles.
- **Round bars, blocks and billets.** Press forged with a recorded reduction ratio.
- **Discs, tube sheets and covers.** Upset forged, solid or trepanned, proof-machined for volumetric inspection.
- **Sleeves and bushings.** Bored on the CNC deep-hole drilling machine, to 1,600 mm diameter by 10,000 mm.
- **Forged pipes and hollow bars.** Trepanned or mandrel forged from solid blanks.
- **Valve and wellhead parts.** Stems, seat rings, bodies, bonnets, blocks and spools.
- **Gears, rolls, wheels and nozzles.** Near-net open-die shapes to drawing.

Delivery condition: as-forged with allowance, rough or proof machined, or finish machined to drawing, in condition A or aged to RH950, H950, H1000, H1025, H1050, H1100, H1150 or H1150M.

## 9. Plant and working envelope

| Step | Equipment | Limit |
|---|---|---|
| Melting | 25 t electric arc furnace, 25 t and 50 t ladle furnaces, 30 t and 60 t vacuum oxygen decarburisation | 60 t maximum heat |
| Remelting | 3 t and 6 t protective-atmosphere electroslag, 6 t vacuum arc remelting, 3 t vacuum induction melting | Double-melt routes without subcontracting |
| Forging | Hydraulic presses at 6,300 t, 4,000 t and 2,000 t; hammers 750 kg to 5 t | 30 t heaviest single piece |
| Ring rolling | Radial-axial mills at 6 m, 3 m and 1 m | OD 50 mm to 6,000 mm |
| Heat treatment | 14 furnaces, car-bottom to 8,000 x 2,000 x 2,000 mm, two 15 m well-type | Vertical quench for long shafts |
| Machining | Vertical lathes to 5,000 mm swing, horizontal lathes to 14 m between centres, deep-hole drilling to 1,600 x 10,000 mm | Finish machining in house |

These are plant limits, not grade limits. For 1.4534 the practical envelope is set case by case by the ingot available from the remelting route and by quenching the section uniformly.

## 10. Where the grade is used

- **Subsea and wellhead.** Deepwater production components, wellhead and Christmas-tree parts, valve stems and seat rings for ball, gate, globe, check and plug valves.
- **Aerospace.** Landing-gear parts, structural sections, pins and shafts, normally ordered to AMS 5629.
- **Rotating equipment.** Turbine and compressor rings and shafts, gearbox parts, power-transmission spindles, air compressors, generator components.
- **Chemical and petrochemical.** Chemical and plunger pump shafts and rings, pressure-vessel and heat-exchanger flanges, tube sheets and forged pipe, column and tower internals.
- **Nuclear.** Components needing stress-corrosion cracking resistance with high proof strength.
- **Heavy machinery.** Mill and mixer parts, crystalliser equipment, forged rolls and wheels for shipbuilding, pulp and paper and pharmaceutical plant.

## 11. Testing and certification

| Test | Equipment | Standard |
|---|---|---|
| Chemical analysis | SPECTROTEST TXC25 optical emission spectrometer | ASTM E415 |
| Carbon and sulphur | HIR-9440D infrared analyser | ASTM E1019 |
| Alloy verification | X-Mwt3000TX handheld analyser | Positive material identification |
| Tensile | WE-600B 600 kN, WDW-300 electronic | ASTM A370, ISO 6892 |
| Impact | JBN-300 pendulum with DWC-60 bath | ASTM A370, to minus 60 C |
| Hardness | TH140 Leeb tester | ASTM A956, converted per ASTM E140 |
| Ultrasonic | PXUT-3300, USM35XS, CTS-22 | ASTM A388, EN 10228-3, SEP 1921 |
| Magnetic particle | CYE-3A crack detector | ASTM E709 |
| Grain size and structure | XJP-6A microscope with mounting and polishing line | ASTM E112 |

EN 10204 3.1 mill certificates are issued as standard. EN 10204 3.2 witnessed by BV, DNV, LR, SGS, TUV or the customer's own inspector is available on request. Intergranular corrosion testing to ASTM A262 or G28, pitting tests to ASTM G48 and impact testing below minus 60 C are placed with an accredited laboratory and reported alongside the mill certificate.

## 12. Questions buyers ask

### What is X3CrNiMoAl13-8-2?

A martensitic precipitation-hardening stainless steel, EN 1.4534, with 12.25 to 13.25 per cent chromium, 7.5 to 8.5 per cent nickel, 2.0 to 2.5 per cent molybdenum and 0.90 to 1.35 per cent aluminium. It is the European designation of UNS S13800, sold as PH 13-8 Mo and covered by ASTM XM-13 and AMS 5629.

### Is it the same as PH 13-8 Mo and UNS S13800?

Yes, the same alloy under different names. The EN specification is tighter on two elements: manganese 0.10 per cent maximum against 0.20, and aluminium 0.90 to 1.20 per cent against 0.90 to 1.35. Orders that must meet EN 1.4534 rather than XM-13 should say so, because the melt is aimed at the narrower range.

### Does H900 apply to this grade?

No. H900 is a condition of 17-4 PH. The lowest standard ageing temperature for X3CrNiMoAl13-8-2 is 510 C, giving H950 and RH950. The standard conditions are A, RH950, H950, H1000, H1025, H1050, H1100, H1150 and H1150M. Drawings calling for 13-8 Mo in H900 usually carry over a note written for 17-4 PH.

### How does it compare with 17-4 PH?

1.4534 is held to much lower sulphur and phosphorus and is normally double melted, so it carries better toughness across the grain and better resistance to stress-corrosion cracking, particularly in heavy sections. It also reaches higher strength, 1515 MPa minimum in H950. Against that it machines roughly 20 to 30 per cent slower than 17-4 PH in condition A and costs more per kilo. Where the section is thin and loading is longitudinal, 17-4 PH is often the cheaper answer.

### Which condition should be specified?

H950 or RH950 for maximum strength. H1000 or H1025 for near-peak strength with better toughness, and for service where stress-corrosion cracking governs, since ageing at 538 C or above is the usual recommendation. H1050 to H1100 for a working balance. H1150 or H1150M where toughness and machinability lead. For heavy machining content, order condition A or H1150M and age afterwards.

### Can it be welded?

Yes, by inert-gas shielded and resistance processes, normally in the solution-annealed condition with 13-8 Mo filler, and preheat is not usually needed. Solution treating the welded part before ageing gives the best balance of strength, ductility and corrosion resistance. Material welded in an overaged condition must be re-solution treated before it will respond to ageing.

### What sizes can be forged?

The plant rolls rings to 6,000 mm outside diameter and forges single pieces to 30 tonnes, but for a precipitation-hardening stainless the practical limit comes from the remelted ingot and from quenching the section uniformly. Send outside diameter, bore, height and finished weight, or the drawing, and the size is confirmed with the quotation. Minimum order 10 kg, no minimum piece count.

### What is needed for a firm price?

Grade and specification; dimensions or a drawing in PDF, DWG, DXF or STEP; quantity and expected repeat volume; delivery condition; heat treatment, testing and NDT acceptance class; certificate type and destination port. With those in the first email a price normally comes back within two working days.

### How long does an order take?

20 to 60 days from order confirmation. This grade sits at the longer end because the low sulphur and phosphorus limits call for a remelting step, and solution treatment plus ageing add furnace time. Witnessed inspection to EN 10204 3.2 and corrosion testing placed outside also need scheduling.

## Contact

**Jiangyin Jiangnan Metal Co., Ltd.**
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China
Telephone, WhatsApp and WeChat: +86 189 2135 9659
Email: sales@steelforgepieces.com
Hours: Monday to Saturday, 08:00 to 17:30 China Standard Time (UTC+8)

---

Compiled by the engineering office of Jiangyin Jiangnan Metal Co., Ltd., an integrated melting works and open-die forging factory in Jiangyin, Jiangsu, China, operating since 1997. Figures are drawn from the published requirements for UNS S13800 and 1.4534 under ASTM A564, ASTM A693 and AMS 5629, together with producer data for PH 13-8 Mo. They are given for selection purposes; the properties that apply to an order are those recorded on its mill certificate. Reviewed 10 October 2026.