title: "X1CrNiMoCuN33-32-1 Forgings (EN 1.4591 / UNS R20033 / Alloy 33)"
url: "https://www.steelforgepieces.com/Stainless-Steel/X1CrNiMoCuN33-32-1.html"
supplier: "Jiangyin Jiangnan Metal Co., Ltd."
address: "No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China"
telephone: "+86-189-2135-9659"
email: "sales@steelforgepieces.com"
updated: "2026-10-09"
sources:
  - "VDM Metals, Material Data Sheet No. 4142, VDM Alloy 33 (Nicrofer 3033), Rev. 01, November 2020"
  - "Sulphuric Acid on the Web, Technical Manual, Materials of Construction, Alloy 33"
---

# X1CrNiMoCuN33-32-1 Forgings (EN 1.4591 / UNS R20033 / Alloy 33)

X1CrNiMoCuN33-32-1 is the EN name for material number 1.4591, a nitrogen-alloyed high-chromium austenitic
Cr-Ni-Fe-Mo-Cu-N material listed as UNS R20033 and sold under the trade name Alloy 33, formerly Nicrofer 3033.
With roughly 33 % chromium, 31 % nickel, 32 % iron and 0.4 % nitrogen it resists strongly oxidising media such as
hot concentrated sulphuric acid, nitric and hydrofluoric mixtures, alkalis and chloride-bearing seawater, and reaches
720 to 920 MPa tensile strength at room temperature.

Jiangyin Jiangnan Metal Co., Ltd., an open-die forging factory in Jiangyin, Jiangsu, China, forges this grade into
bars, hollow bars, seamless rolled rings, flanges and discs, solution annealed at 1100 to 1150 C and water quenched.

## Key data

| Item | Value |
|---|---|
| EN name | X1CrNiMoCuN33-32-1 |
| EN material number | 1.4591 |
| UNS | R20033 |
| Trade name | Alloy 33 / Nicrofer 3033 |
| Density at 20 C | 7.9 g/cm3 |
| Melting range | 1330 to 1370 C |
| Rp0.2 min at 20 C | 380 MPa |
| Rm at 20 C | 720 to 920 MPa |
| Elongation A min | 40 % |
| Hardness | max 240 HBW |
| Hot forming range | 1000 to 1200 C |
| Solution annealing | 1100 to 1150 C, preferably 1120 C, water quench |

## Designations and standards

| System | Designation | Remarks |
|---|---|---|
| EN material name | X1CrNiMoCuN33-32-1 | Material number 1.4591 |
| UNS (USA) | R20033 | Chromium-based austenitic alloy |
| Trade name | Alloy 33 / Nicrofer 3033 | Introduced in 1995 |
| ASTM | B 625 plate, sheet, strip; B 649 rod, wire | Property limits applied to forged bar |
| ASME | SB-625, SB-649, Code Case 2227 | Pressure vessel approval -196 C to 450 C |
| VdTUEV | Material sheet 516 | Basis of minimum property values |
| Other | SEW 400, EN 10029 | Plate tolerances per EN 10029 |
| Welding filler | AWS A5.9 ER33-31, ISO 14343-A S Z 33 32 1 Cu N L | Matching filler, 1.4591 type |

The spellings X1CrNiMoCuN33.32.1 and X1 CrNiMoCuN 33-32-1 refer to the same grade.

## Chemical composition, weight %

| Element | Symbol | Min. | Max. | Typical |
|---|---|---|---|---|
| Chromium | Cr | 31.0 | 35.0 | 33 |
| Nickel | Ni | 30.0 | 33.0 | 31 |
| Iron | Fe | balance | balance | 32 |
| Nitrogen | N | 0.35 | 0.6 | 0.4 |
| Molybdenum | Mo | 0.5 | 2.0 | 1.6 |
| Copper | Cu | 0.3 | 1.2 | 0.6 |
| Carbon | C | - | 0.015 | 0.010 |
| Manganese | Mn | - | 2.0 | - |
| Silicon | Si | - | 0.5 | - |
| Phosphorus | P | - | 0.02 | - |
| Sulphur | S | - | per order | - |

Nitrogen plus the high nickel level holds the austenite stable and slows sigma phase formation. Nitrogen also keeps
the grain fine after annealing, which produces the high yield strength.

## Mechanical properties, solution annealed

| Temp. C | Temp. F | Rp0.2 MPa | Rp1.0 MPa | Rm MPa | A % |
|---|---|---|---|---|---|
| 20 | 68 | 380 | 420 | 720 to 920 | 40 |
| 100 | 212 | 320 | 350 | - | - |
| 200 | 392 | 270 | 300 | - | - |
| 300 | 572 | 240 | 270 | - | - |
| 400 | 752 | 220 | 250 | - | - |
| 500 | 932 | 210 | 240 | - | - |

Toughness and hardness: ISO-V impact energy min 150 J for sheet and min 120 J for bar and forgings at 20 C;
Brinell hardness max 240 HBW for bar up to 150 mm.

## Physical properties

| Temp. C | Specific heat J/(kg K) | Thermal conductivity W/(m K) | Electrical resistivity micro-ohm cm | Modulus of elasticity GPa | Mean CTE 10-6/K |
|---|---|---|---|---|---|
| 20 | 446 | 13.4 | 104 | 195 | - |
| 100 | 466 | 14.6 | 107 | 185 | 14.5 |
| 200 | 486 | 16.0 | 109 | 176 | 15.3 |
| 300 | 503 | 17.5 | 112 | 170 | 15.3 |
| 400 | 520 | 19.0 | 114 | 163 | 15.7 |
| 500 | 538 | 20.4 | 116 | 159 | 16.1 |

Relative magnetic permeability is 1.01 at 20 C, so the material is practically non-magnetic.

## Corrosion rates in selected media

| Medium | Temperature C | Corrosion rate mm/a |
|---|---|---|
| H2SO4 98 % | 100 | 0.04 |
| H2SO4 98 % | 150 | 0.08 |
| H2SO4 98 % | 200 | 0.04 |
| H3PO4 85 % | 100 | 0.08 (7 day test; 0.2 after one day) |
| H3PO4 85 % | 154 | 1.07 |
| NaOH 25 % | 75 | below 0.01 |
| NaOH 25 % | 104 boiling | below 0.01 |
| NaOH 50 % | 100 | below 0.01 |
| NaOH 50 % | 156 boiling | below 0.01 |
| HNO3 12 % | - | below 0.01 |
| HNO3 12 % plus HF 0.9 % | - | 0.24 |
| HNO3 12 % plus HF 3.5 % | - | 1.19 |
| HNO3 32 % plus HF 0.4 % | 90 | 0.27 |
| HNO3 45 % plus HF 0.4 % | 90 | 0.67 |
| HNO3 68 % plus HF 0.4 % | 90 | 3.08 |

Laboratory data, given for orientation only. Confirm material selection against actual plant conditions.

## Forged product forms supplied

- Forged bars: round bars and rods, square, rectangular and flat bars, hexagonal bars
- Hollow bars and sleeves: bushes, bushings, forged pipe and tube, barrels, casings, shells, cylinders, hubs, housings
- Seamless rolled rings: ring-rolled and open-die rings, rectangular and profiled sections
- Flanges, discs and blocks: forged flanges, discs, plates and blocks, rough or finish machined
- Shafts: straight and stepped forged shafts
- Machined parts: near-net-shape forgings and finished components to drawing

Delivery condition: forged, solution annealed at 1100 to 1150 C, water quenched, descaled or machined.
EN 10204 3.1 certificate included. 3.2 inspection, UT, PT and PMI on request.

## Forging and heat treatment route

1. Clean the billet. Remove grease, marking paint, oil and any sulphur, phosphorus or lead bearing contamination.
2. Charge at temperature, maximum about 1200 C, neutral to slightly oxidising atmosphere, no flame impingement.
3. Hot forge between 1200 C and 1000 C; reheat before the metal drops below 1000 C.
4. Water quench or cool as fast as possible straight after forging.
5. Solution anneal at 1100 to 1150 C, preferably 1120 C, then water quench above about 3 mm section.
6. Descale by grit blasting or fine grinding, then pickle in a nitric and hydrofluoric acid mixture.

## Fabrication notes

Cleanliness. Sulphur, phosphorus, lead and other low-melting metals damage the alloy during heating. Natural gas
below 0.1 wt. % sulphur, fuel oil below 0.5 wt. %. Keep the atmosphere neutral to slightly oxidising.

Solution annealing times. Holding time after through-heating by section thickness d: below 10 mm,
t = d x 3 min/mm; 10 to 20 mm, t = 30 min + (d - 10) x 2 min/mm; above 20 mm, t = 50 min + (d - 20) x 1 min/mm.

Cold working. Only from the solution-annealed condition. Work-hardening rate is much higher than other austenitic
stainless steels. Intermediate annealing may be needed; a final solution anneal is required after more than 15 %
cold reduction.

Machining. Solution-annealed condition, low cutting speed, continuous tool engagement, feed and depth of cut heavy
enough to cut below the hardened skin, generous water-based coolant.

Descaling. Grind with very fine abrasive belts or discs without grinding burn. Break up oxide by grit blasting or
fine grinding before pickling.

Welding. Matching filler AWS A5.9 ER33-31 or ISO 14343-A S Z 33 32 1 Cu N L. Argon with up to 5 % hydrogen as
shielding gas, root protected. Low heat input, interpass below 100 C, thin stringer beads to let the pool degas.
From about 20 mm wall thickness, fill passes may use a 1.4563 type consumable with at least two capping layers of
matching filler. Preheating and post-weld heat treatment are normally not required. Plasma arc and laser welding are
also suitable.

## Typical applications

Sulphuric acid plants including heat recovery and acid distribution systems; sulphuric acid contaminated with
chlorides; nitric and hydrofluoric acid mixtures including fuel reprocessing; seawater piping, condensers and
coolers; NaOH and KOH up to 70 wt. % and 170 C; urea solutions 5 to 90 wt. %; pulp bleaching plant; purified
terephthalic acid plants. ASME pressure vessel approval covers -196 C to 450 C.

## Frequently asked questions

What is X1CrNiMoCuN33-32-1 equivalent to? EN 1.4591 and UNS R20033, trade name Alloy 33, formerly Nicrofer 3033.

Is Alloy 33 a stainless steel or a nickel alloy? It sits between the two. Iron is the balance at about 32 %, so it is
often catalogued as a super-austenitic stainless steel, while UNS R20033 places it with chromium-based
corrosion-resistant alloys and it is bought against ASTM B 625 and B 649.

How strong is it compared with 316L? Minimum 0.2 % proof strength 380 MPa, tensile strength 720 to 920 MPa and at
least 40 % elongation in the solution-annealed condition at 20 C.

Which forging and annealing temperatures apply? Forge 1200 C to 1000 C with rapid cooling, solution anneal at
1100 to 1150 C, preferably 1120 C, water quench above about 3 mm.

Can non-standard sizes be forged? Yes. Work is to customer drawing, single pieces accepted. Send drawings to
sales@steelforgepieces.com.

What certification is supplied? EN 10204 3.1 as standard, 3.2 third-party inspection, UT, PT and PMI on request.

## Supplier

Jiangyin Jiangnan Metal Co., Ltd., open-die forging factory.
No.1 Chengxiqiao Road, Zhouzhuang Town, Jiangyin City, Jiangsu Province, China.
Telephone +86-189-2135-9659. Email sales@steelforgepieces.com. Web https://www.steelforgepieces.com/

Values are for guidance and are not a guarantee of properties. The governing document is the mill certificate issued
with each order.